Re: [MW:36131] APPROVED WPS IN 2G POSITION BUT PRODUCTION WANT TO DO 5G/6G POSITION USING ASME 2G WPS

Hai,

Please note that welding positions for procedure qualification is a non essential variable.
(in the Previous asme sec IX Editions, addition of position was a supplementary essential variable which is applicable only if toughness requirments applicable)

So if you qualify the PQR in any positions will qualify all positions.(for the welding process like GTAW, SMAW, FCAW, GMAW & SAW).

Regarding the performance qualifications, positions qualifications shall follow ASME section IX table QW 461.9.


With Regards,

SANDEEP RAGHAVAN







On Tue, 28 Jul 2026 at 5:43 PM Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
For WPS, welding position is not an essential variable unless there is a requirement for Toughness. For Welders , Welding Position is an essential variable. 
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 1090 & EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Mon, Jul 27, 2026 at 9:12 PM Bharath Kumar <vbmkumar1988@gmail.com> wrote:
Hi,

you need to verify whether the supporting PQR for that WPS qualifies all required positions, the welding position used for PQR can be an essential variable for some welding processes. If the PQR was qualified only in 2G, it does not qualify the WPS for all welding positions. You must check the applicable essential variables for the specific welding process in ASME sec IX . 

BR
V.bharath

On Sat, Jul 25, 2026, 1:51 PM Dominant QC <dominantqc@gmail.com> wrote:
Dear experts,

My contractors wants to use approved 2G position WPS for production joints which in 5G/6g position other than 2G position and WQT for 6G position. References to ASME. Can we proceed to do that or do we need to use approved WPS in 6G/ALL positions?

Regards,
Sya

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/a2026e50-8b41-42a7-bd00-1852f82aa1ean%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAERJn6C7YFVccc0S7WS8%2Bc1-birn%3Dfyor2hiu6Qm7OQ-rdmYNA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eP3EBUhCWahuWbtkZ5X2GjDo0BxM4kroDzhm-bmeNXKNQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAFBEtQpy06Ara1WEE7R0G4%3DkJ6qxmunaP207H66Hz2K9pPc8mQ%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...