Hi,

For your case less than 5 mm, i agree with Mr.Nor Ahmad, he has the explicit reply.

Thanks.
Mohamed Muneeb Mahaboob.
 
Date: 2019-07-18 12:03
Subject: Re: [MW:29863] Asme Section IX Thickness range qualification
Dear Isac,

There are two type of thickness as per ASME IX i.e. base metal thickness, "T" and weld metal thickness, "t". WPS was qualified using 25.4 mm pipe (test specimen). The test specimen was welded by GTAW and SMAW welding process. The test specimen was welded by GTAW up to thickness of deposited 8mm and followed by SMAW  on the remaining thickness i.e. 16.5mm. So t for GTAW is 8mm and t for SMAW is 16.5mm. Therefore, the range thickness qualified as per QW-451 for base metal (T) and weld metal (t) as follows:

1. Base metal thickness, T: range of thickness qualified (for test specimen thickness of 19mm to 38mm) are 5 mm Min. to 2T (2 x 25.4 = 50.8mm) Max. However, if your WPS/PQR with impact test, the range base metal thickness qualified is T or 16mm, whichever is less as per QW-403,6. For test specimen thickness 25.4mm, T qualified is 16mm to 50.8mm only.

2. Weld metal thickness, t:
    a) weld metal thickness qualified for GTAW is 2t = 2 x 8 = 16mm. Max
    b) weld metal thickness qualified for SMAW is 2t = 2 x 16.5 = 33mm Max.

Your question: Can I make a weld using only the GTAW process, base metal with a thickness of less than 5mm? 
The answer is NO because the minimum base metal thickness qualified is less than 5mm either by GTAW or SMAW process.





However, there little bit difference on converting between imperial unit and metric unit. If we you calculate 3/16in. x 25.4 = 4.8mm but ASME IX use 5 mm. This depend on unit is used for your design/project.

Thanks & regards.

Mohd Nor

On Thursday, 18 July 2019, 11:04:04 am GMT+8, Isac Passaura <isac.passaura@gmail.com> wrote:


Thanks for the feedback

Yes, snap is ready WPS, follows attached.

But according to QW-451 because the coupon thickness is 25.4mm, the qualified range would be 5 to 2T, regardless of having deposited only 8mm with the GTAW process?

Thanks.

Isac

Em quarta-feira, 17 de julho de 2019 04:37:57 UTC-3, Muneeb escreveu:
Yes you can, 

Your 25.4 mm with gtaw and smaw can write 2t ranges from your PQR for what has been deposited individually.

you are going to write a WPS or below snap is ready WPS?

Check impact / PWHT requirements for what you qualified and what recommended in production joint.

Thanks.
Mohamed Muneeb Mahaboob.
 
Date: 2019-07-17 04:25
Subject: [MW:29843] Asme Section IX Thickness range qualification
Dear Experts,

I have some difficulty to interpret the requirements of ASME section IX

I have a  PQR Based on a dual process GTAW+SMAW ( 8 mm+17,4 mm) on an 25,4 mm butt weld.

Can I make a weld using only the GTAW process, base metal with a thickness of less than 5mm?

Are the image conditions correct?


wps77.png


Please give with details explanation regarding my above difficulty.


Thanks and Regards


Isac







--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ c74dd763-9499-4097-b2cc- 5cd52a84818d%40googlegroups. com.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/973f737e-654a-43df-bf63-f84ed582caa9%40googlegroups.com.

For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/145011575.3598594.1563426218112%40mail.yahoo.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...