Hi,

There are two ways to approach this problem, 

1) To go strictly by codes & standards, ASME (Sec IX)for welding does not consider chemical composition of weld metal as essential variable, so as long as the weldment passes tensile, bend & impact(if toughness is required) tests, the weldment is acceptable. Note that for weld overlay, Chemical composition is an essential variable.

2) If the application environment  of the product is susceptible to pitting corrosion, then it is a problem that needs to be rectified.  Possible reasons may be migration/segregation of Mo towards any of the base metal because of improper welding parameter/procedure used. Performing a chemical analysis across the welded specimen can possibly be a first step in identifying the root cause for this problem.

Regards,
Bala.


On Sunday, August 20, 2017 at 6:52:08 PM UTC+5:30, biju wrote:
Hi,
We have a to weld a 316L pipe to F347 flange using 316L electrode.after welding during PMI it has been noted that Mo content in weld metal is only 0.15--0.21 range.Is there any document which specifies how much dilution can be acceptable

Biju
Sent from my iPad

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...