RE: [MW:23630] RE: 23626] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

I definitely agree with the below statement.

From corrosion testing we have performed on 316L and 2101 duplex the HAZ on these welds are very prone to pitting and crevice corrosion due to austenite and ferrite balance.

Heat input is critical.

The elevated temperatures are definitely a factor in the corrosion equation.

With the environment  carbon pickup is definitely a factor.

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimprice@polarcorp.com

 

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Alan Denney
Sent: Wednesday, September 30, 2015 6:44 AM
To: materials-welding@googlegroups.com
Subject: [MW:23629] RE: 23626] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

 

From this I understand that it is a 316L vessel which is exposed in an offshore marine environment and has a nominal operating temperature of up to 40 degrees C and after 5 years exposure is showing signs of external pitting corrosion. I believe the reason why this has occurred is straightforward; it is operating at a temperature and in an environment where pitting is inevitable. The critical pitting temperature of 31L stainless steel is about 15 degrees C in a chloride bearing environment for solution treated 316L. Although 316L is used in marine environments it performs without pitting only at moderate temperatures [and even at moderate temperatures it will show signs of corrosion in crevices] . I also suspect the steel temperature may be higher than the greatest ambient/operating temperature of 40 deg C due to solar gain, which makes the situation worse. Alongside the welds you may be suffering crevice corrosion. Iron contamination could also be a factor particularly with some of those surface lines away from welds due to contact with carbon steel materials.

 

In my view it comes down to understanding the environment in which the material is to be exposed, (marine and high temperature relative to CPT) and the limitations of 316 stainless steel. There is a lot of information on the web if you do a search. The material selection is hence wrong for the external environment, or the tank should have been painted – yes you do paint stainless steel!

 

Alan Denney

AKD Materials Consulting Ltd

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com]
Sent: 30 September 2015 10:55
To: pgoswami <pgoswami@quickclic.net>
Cc: <materials-welding@googlegroups.com> <materials-welding@googlegroups.com>
Subject: [MW:23626] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

 

Dear Sir,

 

It's is a corrosion inhibitor storage tank for subsea pipeline project , 

 

operating temperature is 40degree Celsius ,

Operating pressure.     Is .7KPA

Chemical is injected inside the tank , as per design data sheet there is no insulation.

 

Now I have planned to visit the location and provide more information in environmental condition,

Almost 5years completed and dispatched the job.

P.NEILASHKUMAR 

Sent from my iPad

MOB : 966 533098265

            91+9952110791


On Sep 30, 2015, at 5:27 AM, pgoswami <pgoswami@quickclic.net> wrote:

Hi Neileshkumar,

What're the surrounding operating or environmental conditions around the tank. Are there any acid fumes involved. Looks like this tank was not insulated at all??? Is that true.

Appreciate more information on the operating conditions.

 

Thanks


 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineering Specialist
Hamilton, Ontario, Canada
pgoswami@quickclic.net
pradip.goswami@gmail.com
ca.linkedin.com/pub/pradip-goswami/5/985/299

-----Original Message-----
From: Neilash Kumar [mailto:neilashkumar@yahoo.com]
Sent: Tuesday, September 29, 2015 2:45 AM
To: Pgosami Sir; Pgosami sir
Subject: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

Dear Sir,

Good Morning, please find the attached tank drawing fabricated by us for our client & it is corroded fully , Can you please clarify,

1. Why the tank are corroded So fast?
2. Can you please advise us the method to stop /reduce the rate of corrosion by applying a top coat &  what type of coating to be applied?

please advise me . Material is 316L tank.

Regards
P.Neilashkumar

<Tank Corrosion.pdf>

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/81B20544-18A9-45D3-81A3-EDB56129B98A%40yahoo.com.
For more options, visit https://groups.google.com/d/optout.

 

This email has been scanned by BullGuard antivirus protection.

For more info visit www.bullguard.com

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/000001d0fb75%243f7b6060%24be722120%24%40denney1.freeserve.co.uk.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...