Yes you can ,directly go for passivation process if there is no pitting corrosion observed .
Regards
Shyamal
Sent from my iPhone
Sent from my iPhone
Picking would remove contaminants (iron)Sent from my BlackBerry 10 smartphone.
From: NeilashkumarSent: Τρίτη, 29 Σεπτεμβρίου 2015 - 19:14To: George H DilintasCc: Welding GroupsSubject: Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGDThis message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com --Dear sir ,Thanks for your answer , now I have doubt instead of pickling spray can I go directly to passivation spray followed by rinsing and cleaning. I need your advise and procedures if any?
P.NEILASHKUMARSent from my iPadMOB : 966 53309826591+9952110791It looks like iron contamination.
Actions to implement:
- Removal of rust by stainless steel compatible brushes/disks.
- Pickling
- Avoid contact with carbon steel tools, jigs etc
best regards
Dr. Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE
Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04
Neilash Kumar ---29/09/2015 09:56:39--- Dear Sir, Good Morning, please find the attached tank drawing
From: Neilash Kumar <neilashkumar@yahoo.com>
To: George H Dilintas/GRC/VERITAS@VERITAS, Welding Groups <materials-welding@googlegroups.com>
Date: 29/09/2015 09:56
Subject: NEED ADVISE CORROSION IN INHIBITOR TANK REGD
Dear Sir,
Good Morning, please find the attached tank drawing
fabricated by us for our client & it is corroded fully ,
Can you please clarify,
1. Why the tank are corroded So fast?
2. Can you please advise us the method to stop /reduce the rate of corrosion by applying a top coat & what
type of coating to be applied?
please advise me . Material is 316L tank.
Regards
P.Neilashkumar[attachment "20150909_102338.jpg" deleted by George H Dilintas/GRC/VERITAS] [attachment "20150909_102358.jpg" deleted by George H Dilintas/GRC/VERITAS]
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF57240EB1.3777AADA-ONC1257ECF.005C9F78-1443545501800%40LocalDomain.
For more options, visit https://groups.google.com/d/optout.
<graycol.gif>
Comments