[MW:23584] Re: NEED ADVISE CORROSION IN INHIBITOR TANK REGD

It looks like iron contamination.
Actions to implement:

  1. Removal of rust by stainless steel compatible brushes/disks.
  2. Pickling
  3. Avoid contact with carbon steel tools, jigs etc

best regards

Dr. Georgios Dilintas

Authorized Nuclear Inspector
Authorized Inspector Supervisor

I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS PIRAEUS - GREECE

Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04


Neilash Kumar ---29/09/2015 09:56:39--- Dear Sir, Good Morning, please find the attached tank drawing

From: Neilash Kumar <neilashkumar@yahoo.com>
To: George H Dilintas/GRC/VERITAS@VERITAS, Welding Groups <materials-welding@googlegroups.com>
Date: 29/09/2015 09:56
Subject: NEED ADVISE CORROSION IN INHIBITOR TANK REGD




 Dear Sir,

Good Morning, please find the attached tank drawing
fabricated by us for our client & it is corroded fully ,
Can you please clarify,
1. Why the tank are corroded So fast?
2. Can you please advise us the method to stop /reduce the rate of corrosion by applying a top coat &  what
type of coating to be applied?

please advise me . Material is 316L tank.

Regards
P.Neilashkumar[attachment "20150909_102338.jpg" deleted by George H Dilintas/GRC/VERITAS] [attachment "20150909_102358.jpg" deleted by George H Dilintas/GRC/VERITAS]

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...