Re: [MW:13969] WELDING OF SA 240 310S

Hi!
SS310 material is Nil fe rrite  and having  a tendancy of Fissures /hot crack
 
therefore welding is very critical  preferably you should weld with Low Heat /interpass and use smaller bead head with use of smaller dia consumables
Regards
 
Hegde P.B.
08805593046

--- On Wed, 21/3/12, Mukesh Chaudhari <mukesh.chaudhari@orientalindia.net> wrote:
 
From: Mukesh Chaudhari <mukesh.chaudhari@orientalindia.net>
Subject: [MW:13965] WELDING OF SA 240 310S
To: materials-welding@googlegroups.com
Date: Wednesday, 21 March, 2012, 6:43 PM

 

Hi all,

We facing problem to weld SA240 310S material. We found linier indication(crack) in Radiography testing.

Once the repair comes then after repair we found more liner indication.

 

Thanks & Regards,

Mukesh Chaudhari
Sr. Engineer Quality

Oriental Manufacturers Private Limited
A: P.C.C. Notified Area, Ranoli Station Road,

 Ranoli -391 350 Baroda Gujarat India

T: +91.265.223 1663/2232936

F: +91.265.223 0171
E:  mukesh.chaudhari@orientalindia.net 
W: http://www.orientalmanufacturers.com

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...