Re: [MW:13955] use of E 7018 -1 & ER 70S-6 to weld SA 516 GR 70 MATERIAL

Dear all,

You can not use ER70S-6 for GTAW welding since it contains higher Si content than ER70S-2. ER70S-6 can be used if your shielding is by CO2 (i.e. in GMAW process). Purpose of addition of si is to flux o2 from weld when co2 is used as shielding.

Regard,

Maulik Thakkar
Welding Engineer

On Tue, Mar 20, 2012 at 10:34 PM, Maulik Thakkar <mlkthakkar2@gmail.com> wrote:
Dear all,

You can not use ER70S-6 for GTAW welding since it contains higher Si content than ER70S-2. ER70S-6 can be used if your shielding is by CO2 (i.e. in GMAW process). Purpose of addition of si is to flux o2 from weld when co2 is used as shielding.



On Tue, Mar 20, 2012 at 3:32 PM, Kavin Murugam <kavin202082@yahoo.com> wrote:
Dear Asrad Azmi,
Additional to Mr. Arunachalam's comments
 
F7P8 EH12K (P= with PWHT) / essential variables as per QW404.9
 
Kavin Murugam
0126159644

From: Arunachalam A <arunvani@gmail.com>
To: materials-welding@googlegroups.com
Sent: Sunday, March 18, 2012 12:04 AM
Subject: Re: [MW:13913] use of E 7018 -1 & ER 70S-6 to weld SA 516 GR 70 MATERIAL

ER 70-S6 weld metal chemical analysis does not meet A No. 1.  

If you have qualified a WPS with Er 70-S3 etc, then this wire is not acceptable.  ( Manganese content is more than 1.6% in weld metal)

arun

On Sat, Mar 17, 2012 at 12:23 PM, asad azmi <azmiasadayub@gmail.com> wrote:
Dear All,
 
Vessel is being fabricated as per ASME SEC VIII DIV 1.
 
Base material - SA 516 GR 70 HIC - 30 mm Thk. IMPACT TEST not required.
 
  
normally  we are using E 7018 for SMAW,  ER 70S2 for GTAW  & F7P8 EH12K  for SAW Process to weld  above base material.
 
Can we use E7018-1 for SMAW,  ER 70 S6   for GTAW  & F7P8 EH12K for SAW for the above base material.
 
Please Advice.
 
Thanks & Regards
 
Asad Azmi
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Arunachalam.A,

Give a Man some Money, you make him Beggar for a Day.
Make him live on Welfare schemes, you succeeded in making him Beggar for life.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...