ASME Second VIII Div 1 permits use of backing strip for the type of joint in question. Please refer para UW-12 for joint efficiency.

But why the contractor is not prefering a single side full penetration joint configuation or even a double welded butt joint. Welding from inside is not a big issue for 600 dia shell.

RT with backing strip in position may be a bit tricky and interpretation problematic due to slag entrapment between shell and b/s.

Gopu
Sent from BlackBerry® on Airtel

From: prem nautiyal <prem_nautiyal26@yahoo.com>
Sender: materials-welding@googlegroups.com
Date: Tue, 20 Mar 2012 00:19:33 -0700 (PDT)
To: <materials-welding@googlegroups.com>
ReplyTo: materials-welding@googlegroups.com
Subject: [MW:13932] Backing strip

Hello friends
 
Need expert opinion on the subject as follows..
 
A Heat exchanger is being fabricated as per ASME Sec VIII Div.1.
The Channel Shell and dish end thickness is @ 10mm and dia. @ 600mm. The MOC is SA516 Gr.70.
Now for the closing joint seam i.e. Channel Shell # Dish end (single V joint) can a "Permanent Backing strip" with 8mm root gap be used ? The permanent backing strip will be 6mm thicknes X 25mm wide and stich fillet welded from inside. Contractor has submitted WPS mentioning permanent backing strip for this joint. Can we accept this ? Is there any provision in code for non-usage of permanent backing strips in pressure parts ?
The joint calls for full radiography. Contractor claims that upto 10mm thickness the RT will be cleared.
Can we accept this case as per ASME Sec.VIII Div.1.
 
Regards
 
Prem Nautiyal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...