[MW:13965] RE: 13963] TENSILE TEST REQUIRMENT FOR PLATES AFTER SIMULATION HEAT TREATMENT

Hi

 

// Plate condition - Plate Hot Rolled//

 

Whether it is from coil or as rolled condition. Hot rolled or cold rolled is a method used to form the plates. It is not the condition of the plate.

Usually the plates will be cast in to slabs and rolled subsequently to either plates cut to the length or made to coils.

 

The plates will have

 

-          Heat no (chemistry from slab while pouring)

-          Plate no (for as rolled)

-          Test no (if produced from coils)

If produced from coil- Heat, Plate, Test no will be there. If the plates are cut from coil, then you need to follow SA 516, Clause 1.4.

 

If from as –rolled- Heat no, Plate no will be reported

BR

M.Vijayan

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of asad azmi
Sent: Wednesday, March 21, 2012 2:27 PM
To: materials-welding@googlegroups.com
Subject: [MW:13963] TENSILE TEST REQUIRMENT FOR PLATES AFTER SIMULATION HEAT TREATMENT

 

Dear All,

 

A vessel is being fabricated as per ASME SEC VIII DIV 1.

 

 

Contarctor has received 3 plates ( SA 516 GR 70 N - 30 mm Thk) which are having one heat number and 3 different Plate No. Plate condition - Plate Hot Rolled. plate manufacturer has not done Simulation heat treatment of test coupon.

 

as per Client  Simulation  heat treatment ( 3 pwht cycle) is reuired. 

 

As per SA 20 PARA 11.1.1 One tension test is required for each plate as rolled. as per client requirment any mechanical testing shall be done after all heat treatment.

 

 

Please advice whether one sample from each plate has to undergo simulation heat treatment cycle & Tension test OR one sample out of any 3 plates shall undego simulation heat treatment & Tension Test.( as heat number is same for each 3 plates)

 

Please give code reference.

 

Thanks & Regards

 

Asad Azmi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



This communication and any files transmitted with it are confidential and may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient or the person responsible for delivering it to the intended recipient(s), please note that any form of distribution, copying or use of this communication or information contained in it is strictly prohibited and may be unlawful. If you have received this communication in error please return it to the sender, and delete the material from any computer. We reserve the right to monitor email communications through normal internal and external networks. We believe but not warrant that the email and the attachments are virus free. The statement and opinions expressed in this communication are those of the writer and do not necessarily represent those of Madina Group, whose registered office address is

P.O. Box 20459, Doha, Qatar.
Tel. +974 44600818
Fax. +974 44603143

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...