ASTM A 148 is a ferritic-pearlitic carbon steel for cast products. It is used for higher pressures and stress parts like crane wheels,etc..
I think the chemical composition is C=0.4-0.5, Mn=0.4-0.8, Si=0.2-0.5,P&S=max.0.090.
First you should arrest the crack by drilling two holes,remove the crack by hand grinding, ensure crack removal by LPT.
Preheat the job to 250 degrees celcius, Use E7018-1 electrodes,Interpass temp of 250 degrees celcius and weld. After welding cover the job with asbestos cloth for slow cooling.
I am suggesting you this procedure because we had repaired one cast steel of similar composition in the past.
Any suggestions / expert comments are welcome...
Cheers
Prem Nautiyal
Godrej, Mumbai
Cell: 9820313278
On Sun, 12 Oct 2008 greetings wrote :
>Friends,
> Crack observed in casting material ASTM A 148 GR 80-40
>Can any one give the process to rectify the crack (welding electrode,Preheat
>Temp & etc)
>
>Regards
>DST
>
>>
PREM S NAUTIYAL
CELL : 9820313278
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment