Skip to main content

Materails FAQs

Q:
What are equivalents for standard Q 235 B (and Q 235 A) for U-channels?
(asked by: boris.vielhaber@vait.com)

A:
DIN Nr. = 2393 T.2, 2394 T.2, EN 10025
W. Nr. DIN 17007 = 1.0038
Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B)


Q:
What is St DIN 2391 BK material?
(asked by: dmcandrews@automaticstamp.com)

A:
Precision steel tubes, cold-finished/hard.


Q:
What is C.D.W. Boiler Tube?
(asked by: montydude123@yahoo.com)

A:
Cold Drawn Welded Boiler Tube.


Q:
WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE
(asked by: sumeetg84@rediffmail.com)

A:
It is a cheaper stainless steel.


Q:
1) What is the main requirement of DIN 2391?
2) What is the meaning of NBK?
(asked by: magdy_9am@yahoo.com)

A:
1) Precision
2) Annealed, normalized.


Q:
How can I get the details of DIN 2440, DIN 2458, DIN 2391 and DIN 2462?
(asked by: tlsx@nasico.com.vn)

A:
Find it at: http://www.mertl.com and
http://www.google.hr/search?hl=hr&q=DIN+2462&meta=


Q:
Where Can I Get Mechanical Properties For St 35.8 Grade I, St 35.8 Grade II and St 35.8 Grade III?
(asked by: ABOHOSAM1951@YAHOO.COM)

A:
You can get them at http://www.mertl.com/anonymous/info1.pdf


Q:
What is the formula to calculate tube weight?
(asked by: senthil718@yahoo.co.in)

A:
Find it out at Technical Data - http://www.steeltubestrade.net/technical.php


Q:
What is chemical composition for Fe430B and Rst 37-2?
(asked by: enteshari@fghco.com)

A:
Italy UNI 7070 = Fe430B = Germany DIN 17100, St 44-2 = W.Nr. 1.0044
Chemical composition (max. values): C = 0.21%, P = 0.050%, S = 0.050%, N = 0.009%
RSt 37-2 = W.Nr. 1.0038: C = 0.17%, P = 0.050%, S = 0.050%, N = 0.009%


Q:
Please let us know the Chemical and Mechanical Properties of ST 35 Bk?
(asked by: shrikamala@hotmail.com)

A:
St 35 = W.Nr. 1.0308
Chemical composition (maximal values in %)
C = 0.18, Si = 0.35, Mn = 0.40, P = 0.050, S = 0.050, N = 0.007*

Condition of supply
BK = Cold-finished/hard (cold-finished as-drawn)
No heat treatment after the last cold-forming process. The tubes therefore have only low deformability.

Mechanical properties at room temperature
Tensile strength (Rm N/mm2 min.) = 440
Breaking elongation (A5 % min.) = 6

* Depending on P-content N up to max.


Q:
1) What is the chemical composition & mechanical properties of DIN 50049?
2) What is the difference between ASTM standards & ASME standards?
(asked by: vinod@furnacefabrica.com)

A:
1) DIN 50049 describes various certificates. Find out more for various tubes at http://www.mertl.com/englisch/downloads_e.htm
2) Find it out at http://principalmetals.com/glossary/step1.asp and http://principalmetals.com/specifications/step1.asp


Q:
What is Inox steel?
(asked by: jhanfman@harfordsystems.com)

A:
It is stainless steel.


Q: Do you have a list on the web of DIN to ASTM comparisons for steel pipes?
(asked by: sales@pipelineinternational.com)

A:
No, I have not.


Q:
IS THIS TYPE OF GRADE AVAILABLE & WHAT IS THE CHEMICAL AND PHYSICAL DETAILS OF THIS GRADE C.S. SEAMLESS TUBE TO DIN 2391 ST 45.2, BKW?
(asked by: vimal@champaksteel.com)

A:
St 45-2 = W.Nr. 1.0408

Chemical properties:

C% = 0.17 - 0.24, Si% = 0.17 - 0.40, Mn% = 0.35 - 0.65, P% (max.) = 0.050, S% (max.) = 0.050, Cr% (max.) = 0.30, Ni% (max.) = 0.30, Cu% (max.) = 0.30

Tubes acc. DIN 2391 are seamless precision steel tubes in the following conditions:
BK = cold finished (hard)
BKW = cold finished (soft)
GBK = annealed (bright)
NBK = normalized

Mechanical properties (at room temperature):

For BK:
Tension strength = 540 N/mm2 min.
Breaking strength (A5) = 5% min.

For BKW:
Tension strength = 470 N/mm2 min.
Breaking strength (A5) = 8% min.

For GBK:
Tension strength = 390 N/mm2 min.
Breaking strength (A5) = 21% min.

For NBK:
Tension strength = 440 to 570 N/mm2 min.
Upper yield strength = 255 N/mm2 min.
Breaking strength (A5) = 21% min.

See also: http://www.mertl.com/anonymous/info7.pdf and http://www.amtsrl.it/content/view/79/140/


Q:
What is the meaning of ERW steel pipe?
(asked by: hrenterprises00071@yahoo.co.in)

A:
Electric Resistance Welded tubes


Q:
Can you tell me about the Certificates according to EN 10204/3.1.b or to DIN 50049/3.1.b?
(asked by: gtsiminakis@yahoo.gr)

A:
Find it out under Downloads at: http://www.mertl.com


Q:
What are the differences between DIN 2448 & DIN 2458 & DIN 2391? Thanks in advance.
(asked by: mavistar@yahoo.com)

A:
DIN 2448 = Standards for seamless steel tubes sizes
DIN 2458 = Standards for welded steel tubes sizes
DIN 2391 = Standards for seamless precision steel tubes sizes
DIN 2393 = Standards for welded precision steel tubes (with close tolerances) sizes
DIN 2394 = Standards for welded precision steel tubes sizes


Q:
What is equivalent material in ASTM for 1.0038 (RSt 37-2, 1.4301 (V2A), 1.4541 (V2A), 1.4571 (V4A)? Kindly email me.
(asked by: namrata.nagpurkar@gmail.com)

A:
W.Nr. 1.0038 = RSt 37-2 = A 570 Gr. 36
W.Nr. 1.4301 = X 5 CrNi 18 10 = 304, 304 H
W.Nr. 1.4541 = X 6 CrNiTi 18 10 = 321
W.Nr. 1.4571 = X 6 CrNiMoTi 17 12 2 = 316 Ti


Q:
Equivalent in ASTM of BS4360 Grade 43A
(asked by: judyilagan_agp@yahoo.com)

A:
ASTM A36


Q:
What is the equivalent material of 25 CrMo 4 & St 44?
(asked by: rbodiwala@essar.com)

A:
See previous answers to sprit_feng@spritltd.com, onkarnath@sprayindia.com and pelaez_ray@yahoo.com


Q:
Dear Sir, Is ASTM A53B pipes suitable for pumped sewage applications? If not what is the suitable overground piping for the same applications?
(asked by: designer194@yahoo.com)

A:
See answers to johnbritto@knm-group.com and phantomlord_met@yahoo.com


Q:
1) What are the DIN equivalents for ASTM A106, A270, and A312?
2) Is there a place where I can get more cross-ref / comparison info?
(asked by: steve.wetter@enerfab.com)

A:
1) See previous answers to onkarnath@sprayindia.com and wmoore@airinterus.com

2) Yes, it is this page but you have to use Find option in the Edit menu (see title). There are several very useful web sites that you can find through Useful links (e-pipe Co.,Ltd., IranSteelCenter.com, MARYLAND METRICS, Mesteel.com, TubeNet etc.)


Q:
What is AFNOR and kindly tell me the equivalent material for 30 NCD 11 in DIN standards?. Also give me the mechanical properties of 30 NCD 11.
(asked by: dee_ramv@rediffmail.com)

A:
AFNOR are French standards.
30 NCD 11 has not equivalent in DIN standard and I haven't any data of its mechanical properties.


Q:
Dear Sir, we require all material equivalent standard to Indian Standards.
(asked by: mintoindustries@gmail.com)

A:
You can get them at: http://www.bis.org.in/index_home.htm


Q:
Need details on specification DIN 2394 ST - 37.2.
(asked by: jtursky@gjsteel.com)

A:
See previous answers to pelaez_ray@yahoo.com and ginforge@jla.vsnl.net.in


Q:
What is the Equivalent Material for Dillimax 690 and advise if ALDUR700QL equivalent Dillimax 690?
(asked by: ganesan@mauajurong.com.br)

A:
DILLIMAX 690 is high strength fine grained structural steel quenched and tempered.
ALDUR 700 Q, QL, QL1 = S690Q, QL, QL1 acc. EN 10137-2 is equivalent to DILLIMAX 690.

More about it find at: http://66.249.93.104/search?q=cache:dDXEAyizQ30J:www.petrosteel.com/grade_info/DILLIMAX_690.pdf+Dillimax+690&hl=hr and http://66.249.93.104/search?q=cache:6LwOiX_tk6MJ:www.voestalpine.com/servlets/apploader/j910345/AttachmentDownload.jsp%3Fatt%3D3621%26site%3Dvagb%26language%3Dde%26article%3D8233%26session_id%3D80350761079+ALDUR+700+QL&hl=hr


Q:
What is the Hardness and Mechanical Properties for Normalized AISI 4140, SAE 4140 and SCM 440?
(asked by: ganesan@mauajurong.com.br)

A:
Find it out also at: http://www.woodcousa.com/material_req.htm


Q:
Dear sir kindly tell me the material composition for 30 NCD 11 and equivalent material in Indian standards.
(asked by: dee_ramv@rediffmail.com)

A:
AFNOR 30 NCD 11: C = 0.25-0.35%, Si ≤ 0.40%, Mn = 0.20-0.50%, P ≤0.040%, S ≤ 0.035%, Cr = 0.70-1.10%, Mo = 0.25-045%, Ni = 2.70-3.30%.
I have not Indian standards.
See also previous answer to parry_iyer@yahoo.com


Q:
What is the ASTM equivalent for the tube material St 35.8 DIN 17175/III (German Std.)?
(asked by: ranga@ramsis.com.bh)

A:
See previous answer to onkarnath@sprayindia.com


Q:
What is meaning of PSL-1 and PSL-2?
(asked by: ikramshafi@hotmail.com)

A:
See it at: http://www.woodcousa.com/material_req.htm


Q:
What is Indian equivalent of casting 25CrMo4V?
(asked by: forte_ag@rediffmail.com)

A:
See answer to parry_iyer@yahoo.com


Q:
What is the ASTM equivalent for Tube material spec STB 30 (Japanese Std.)?
(asked by: srini@ramsis.com.bh)

A:
I have no data for such kind of steel.


Q:
What is 35c8, 40cr5mo6, 15cr3 grades of steel?
(asked by: dayaram@dantal.in)

A:
35C8 - Carbon steel
40Cr5Mo6 - Alloy Chromium-molybdenum steel
15Cr3 - Chrome steel


Q:
What should be chemical composition (especially B) 19MnB4 DIN1654-4? Thanks!
(asked by: seeciil@yahoo.com)

A:
C = 0.17-0.24%, Mn = 0.80-1.15%, Si = 0.40% (max.), P = 0.035% (max.), S = 0.035% (max.), B = 0.0008-0.005%


Q:
What are you manufacturing?
(asked by: balaganesh_tce@yahoo.co.in)

A:
We are not a manufacturer. We are a web site for pipe and tube logistics trade.

It is a tool that can enable its members to find out much easier potential business partners in tube & pipe industry worldwide.


Q:
To what hardness can ST 52 and ASTM 106 Grade B be hardened?
(asked by: vendeez@vsnl.net)

A:
Something about this topic you can find and ask at: http://www.putzmeister.de/gb/news/presse/1077-1/default.asp


Q:
What is ASTM standard equivalent to DIN 2462 - 1.4510H?
(asked by: bob@sunssteel.com)

A:
AFNOR (France) = Z 8 CT 17
AISI/SAE (U.S.A.) = XM 8, 430 Ti
DIN (Germany) - W.Nr. 1.4510 = X 6 CrTi 17
GOST (Russia) = 08Ch17T
JIS (Japan) = SUS 430 LX
UNE (Spain) = F.3114-X 8 CrTi 17
UNI (Italy) = X 6 CrTi 17


Q:
What is the pressure rating of different scheduled pipes with respect to dia API 5L X52?
(asked by: ikramshafi@hotmail.com)

A:
Ask this question at
Rolf Lycke AS
Fornebuv. 1, P.O. Box 10
Warehouse: Østre Akerv. 64, N-0581 Oslo
N-1324 Lysaker
Norway
http://www.rolflycke.com/
Telephone: 47 23 244200
Fax: 47 23 244201
Email: oslo@rolflycke.com


Q:
Whats the weight per meter of pipe dia 10 inches sch 40 API 5L X52?
(asked by: ikramshafi@hotmail.com)

A:
Find it at http://www.rolflycke.com/Webdesk/documents/Rolf+Lycke+KOPI/Offshore/X52.pdf

You can also reckon it yourself by using following link: http://www.steeltubestrade.net/tech_formulas.php#carb (calculator: Weight reckoning for any carbon steel tube)


Q:
What is the equivalent DIN Number of ASTM A53?
(asked by: hungvinaconex@yahoo.com)

A:
See previous answers to quasiy@yahoo.com and walterkowalski@Univsteel.com


Q:
What is the difference between ST 52 DIN 2391 and ST 52-3 DIN 2391? Await your kind reply!
(asked by: s520j@163.com)

A:
St 52 = W.Nr. 1.0580, Component = % max., C = 0.20, Si = 0.55, Mn = 1.50, P = 0.050, S = 0.050, N = 0.007
St 52.3 = W.Nr. 1.0570, Component = % max., C = 0.22, Si = 0.55, Mn = 1.60, P = 0.040, S = 0.040, Al = (0.020)


Q:
What is the elongation of ASTM A53?
(asked by: minco_wing@minco.net.cn)

A:
See it at: http://www.chicagotube.com/stockbook/pipe/astm_a53.html


Q:
How to complete my login information? Thank you in advance!
(asked by: niehongzhi@gmail.com)

A:
Print out this link http://www.steeltubestrade.net/instructions.php?page=10 and just follow it up!


Q:
What is the grade name of Indian equivalent of AISI304 & INOX CNZ6
(asked by: navin@emkayauto.com)

A:
See previous answer to parry_iyer@yahoo.com


Q:
What is equiavalent ASTM Grade STB-30?
(asked by: suresht@almufaddal.ae)

A:
I have no data for such steel.


Q:
Equivalents for Fe390 hk uni 591, enaw-6082 uni en586-2?
(asked by: salil_bh2002@yahoo.com)

A:
Find it through: http://www.google.com/


Q:
Steel 35 NCD 16?
(asked by: frankontime@yahoo.com)

A:
See answer to: hayzip@yahoo.com


Q:
What does SAF stands for in SAF 2205 grade?
(asked by: quiantzeal@yahoo.com)

A:
See it at: http://www.engineeringtalk.com/news/sdv/sdv115.html


Q:
Grade 100 Cr 6 – DIN 17230??? Chemical composition + Mechanical properties required! Please help me by emailing
(asked by: pipes@chizhi.dp.ua)

A:
DIN 100 Cr 6, W.Nr. 1.3505

Component = Wt. % max.: C = 0.95-1.05, Cr = 1.30-1.65, Cu = 0.25, Mn = 0.20-0.45, Ni = 0.30, P = 0.27, S = 0.20, Si = 0.17-0.37

Mechanical Properties:
Bulk Modulus = 140 GPa = (English) 20300 ksi - Typical for steels
Hardness, Knoop = 875 - Converted from Rockwell C hardness
Hardness, Rockwell C = 62 - quenched in oil from 150°C tempered
Hardness, Rockwell C = 64 - quenched in oil
Hardness, Rockwell C = 64 - quenched in water from 150°C tempered
Hardness, Rockwell C = 66 - quenched in water
Hardness, Vickers = 848 - Converted from Rockwell C hardness
Machinability = 40% - spheroidized annealed and cold drawn. Based on 100% machinability for AISI 1212 steel
Modulus of Elasticity = 210 GPa = (En.) 30500 ksi
Poisson"s Ratio = 0.3 - Calculated
Shear Modulus = 80 GPa = (En.) 11600 ksi - Typical for steel


Q:
What is the Indian standard equivalent of st 37.8?
(asked by: suresh_mecon@rediffmail.com)

A:
It is the same answer as to parry_iyer@yahoo.com


Q:
what is equivalent of st 37 in astm?
(asked by: mehdimirzaee@gmail.com)

A:
See previous answer to walterkowalski@Univsteel.com


Q:
What is EN equivalent to BS 1387 or ASTM A53?
(asked by: wltcang@tm.net.my)

A:
BS 1387 is EN BS 1387 and for ASTM A53 - see previous answers to: hfayez@nets.com.jo, quasiy@yahoo.com & terence.sundgren@eskom.co.za


Q:
1) What is the american equivalent of european P265GH seamless tube?
2) Is there differences between API 5L grB and ASTM A106 grB?
(asked by: nicolas.audebert@afconsult.com)

A:
1) See it at http://www.t-m-handel.de/engl/liefer/liefer8.htm and combine with previously asked questions.
2) See the answers to the same question at http://www.eng-tips.com/viewthread.cfm?qid=30984&page=5


Q:
Pl inform equivalent ASTM spec for CS seamless heat exchanger tubes to JIS 3461 gr STB52S
(asked by: unath@hotmail.com)

A:
Find it at http://www.tataryerson.com/products_details_GC_1.htm and http://www.premiumtubes.com/sitemap.htm


Q:
I want to know the mechanical property of GS-25 CrMo 4V
(asked by: sprit_feng@spritltd.com)

A:
Ask this question at:
PHB Stahlguss GmbH
http://www.phbguss.de/english/set_00/index.htm
phb@phbguss.de


Q:
I need plate properties for St 37.
(asked by: gajeendran17@yahoo.co.in)

A:
See previous question!


Q:
What are the material yield, tensile stress, composition and equivalent ASME material for ST 35.29?
(asked by: johan@rne-eng.co.za)

A:
Tubes in St 35, acc. DIN 1629 are replaced with St 37 (see answer to pelaez_ray@yahoo.com)
St-35-1 (max. %): C = 0.18, Mn = 0.25, P = 0.060, S = 0.060
St 35-3 = W.Nr. 1.0309: C = 0.16, Si = 0.17-0.40, Mn = 0.35-0.65, P = 0.040, S = 0.040, Cr = 0.30, Ni = 0.30, Al = 0.02, Cu = 0.30, Cr + Cu + Ni = 0.70
St 35-5 = W.Nr. 1.0305 = ASTM Gr. A: C = 0.16, Si = 0.17-0.37, Mn = 0.35-0.65, P = 0.040, S = 0.040, Cr = 0.30, Ni = 0.30, Cu = 0.30, Cr + Cu + Ni = 0.70


Q:
What are the differences in chemical and mechanical properties between ASTM A36 and ASTM A105?
(asked by: chwee-hock.lee@sg.prosafe.com)

A:
Find it at: http://atlas.web.cern.ch/Atlas/GROUPS/Shielding/jdmaterial.htm#Tube & http://www.suppliersonline.com/propertypages/A105.asp and compare with previous answer to wmoore@airinterus.com


Q:
I want to know mechanical and thermal properties (mainly conductivity and stresses) of SA-213, SA-178, SA-516, Sa-106.
(asked by: leonele.espinoza@gmail.com)

A:
Find it at: http://www.chicagotube.com/stockbook/boiler/mechanical_properties.html & http://www.cp-industries.com/mechanicalproperties.htm


Q:
Please tell me equivalent ASME material of API 5L Gr.B.
(asked by: ctikiwala@yahoo.co.in)

A:
They are the common Standards. See also http://www.steeltubestrade.net/tech_standards.php


Q:
Is the thickness of SCH XH equal to SCH XS (80) for size 3" A420 and could you please name an admitted document for that?
(asked by: nemati@goldengroup-ep.com)

A: Find it out at:
http://www.laboiler.com/weldcaps1.html
http://www.techstreet.com/cgi-bin/detail?product_id=2739
http://www.key-to-steel.com/Articles/Art24.htm


Q:
Which is the ASTM equivalent material of DIN St 35.8?
(asked by: fashaikh@engro.com)

A:
See previous answer to onkarnath@sprayindia.com


Q:
Please tell me the material composition of 10B21 boron steel, with the tolerance and permissible limits in %age.
(asked by: atonefasteners@rediffmail.com)

A:
I have no data for this steel. If anybody knows it, please help!


Q:
Please let me know what the BS and ASTM equivalent is for German standard ST37?
(asked by: rme@mossnet.co.za)

A:
See previous question!


Q:
What is the equivalent for DIN ST 52 and DIN ST 37 in Japan Standard?
(asked by: JirapongT@siemens.com)

A:
See it at http://www.steeltubestrade.net/tech_standards.php and previous question asked by walterkowalski@Univsteel.com


Q:
What is Indian Standard equivlent of "API-5L-GRAD B- A106"?
(asked by: galaxy@galaxyhk.com)

A:
See previous answer to parry_iyer@yahoo.com


Q: What is the ISO equivalent of the material GS-17CrMo5-5?
(asked by: bpatel@cbw.de)

A:
Steel casting, Symbol GS-17 CrMo 5 5 = W.Nr. 1.7357 = DIN 17245 ~ ISO DP 4991 = C 32


Q: What is AISI equivalent for ASTM A179 grade tube?
(asked by: shri@gearedhydropower.com)

A:
AISI/SAE/ASTM is identical steel group.
See also answer to onkarnath@sprayindia.com.


Q:
What standards are required in the UAE for hollow structural steel sections and conduits?
(asked by: elmallat@batelco.com.bh)

A:
All most known international standards


Q:
WHAT IS THE EQUAL TO St E 36 AND St E 43 STEEL FOR PRESSURE VESSEL IN ASME CODE?
(asked by: FIORENTINI_MA@YAHOO.COM.AR)

A:
See it at http://www.spartanuk.co.uk/temp/quiality_norms2.htm and http://www.trametal.it/test/quiality_norms3.htm


Q:
What is the equavelant material for E235?
(asked by: aziz9300@batelco.com.bh)

A:
See it at http://www.steeltubestrade.net/tech_standards.php


Q:
What is the equivalent for 35 NCD 16 and 38 NCD 4 steel?
(asked by: hayzip@yahoo.com)

A:
35 NCD 16: EN = 36 NiCrMo 16, AFNOR = Y 36 NCD 16, W.Nr. = 1.6773
38 NCD 4 = UNI 2954 = 39 Ni Cr Mo 3: Hardened and tempered steel for screws


Q:
What is ASTM equivalent for the Material P265GH EN 10028/2?
(asked by: ratha@expg.com.my)

A:
ASME 516 Gr.60/ASME SEC. 2 part A


Q:
What are the mechanical properties of SAE 1010?
(asked by: bharatj@tataficosa.com)

A:
Steel, SAE 1010: Conductivity W/m-C = 59.0, Density kg/m³ = 7.832E+3, Specific Heat J/kg-C = 434.0
Steel, SAE 1010, Sheet: Conductivity W/m-C = 63.9, Density kg/m³ = 7.832E+3, Specific Heat J/kg-C = 434.0
No other mechanical properties specified (elongation, tensile & yield strength etc.)


Q:
What is the thermal conductivity for, din 2448 st 35?
(asked by: mathias.karlsson@ha.aland.fi)

A:
There is no tubes standard that regulates delivery conditions which requires thermal conductivity factor for any pipe. If you need these tubes for some special applications, where it is required, you will have to find either a tube manufacturer or some specialized laboratory that will be able to test them appropriately for you.


Q:
What are the mandatory testing requirement for API 5CT L80 Type 1 and P110 pipes?
(asked by: hedaoopoornima@yahoo.co.in)

A:
Hardness reading (max) = 23.0 HRC, Hardness value (max) = 22.0 HRC, Frequency - casing (one quadrant) = 1/100 pipes or per heat, Frequency - couplings (four quadrants) = 1/50 or per heat, Grain size = 7 or finer, Impact toughness testing = room temperature
P110 = IRP high temperature sour service casing grade (seamless process only, maximum permitted sulphur 0.010%, maximum permitted phosphorus 0.020%): 80° C and above
See also: http://www.psc.ca/irps_gtsws/manuals/pdffiles/irp1_final_2005.pdf


Q:
What is the nearest Indian equivalent for DIN 17102 ST E 380 or ASTM A 572-84 GRADE 60?
(asked by: parry_iyer@yahoo.com)

A:
As I have not Indian norms, please ask this question at:

Essar Steel Limited
27 Km. Surat Hazira Road
394270 Hazira/Gujarat/India
http://www.essar.com
Mr. Pranav M. Gajjar - Project Procurement (HAZ)
Phone: 91-261-5582109; 91-9879103968
Fax: 91-261-5582796, 5582105
pgajjar@essar.com

Jindal Group
Corporate Office
Plot NO 30, Sector 44
122 001-Gurgaon/India
Mr. Atul Kumar Sharma - Deputy Manager Exports
Phone: 0091-11-51538389, 25860717
Fax: 0091-11-25744650
asharma@jaguar-intl.com
General Info
Tel: +91-124-2574325,2574326
Fax: +91-124-2574327
Email: contact@jindal.com


Q:
Hi! I´m working on some bearings for a streetcar. The original drawings specify steel EN 10083-2. This steel is expensive and hard to get so I´m searching for a replacement in an other but similar alloy. Got any tips for me? - Rune Arnesen

A:
Comparison data to this norm you can also find on several places on my web site at: http://www.steeltubestrade.net/tech_standards.php

As I am not qualified for bearings I should suggest you to ask this question at:

SKF Group Headquarters
Hornsgatan 1
SE-41550 Göteborg/Sweden
http://www.skf.com/portal/skf/home/skfsites?lang=en
Phone: +46 31 337 10 00
Fax: +46 31 337 28 32
Email: info@skf.com

Zhangjiagang City Yiyang Pipe Producing Co., Ltd.
207, Fumin Road, Tangqiao Town
Cn-215611 Zhangjiagang/Jiangsu/China
http://yiyangzg.en.alibaba.com
Ms. Snow Wu
Phone: 0086-512-58059526
Fax: 0086-512-58433155
Email: weiwen919@hotmail.com; yiyangfr@163.com

(asked by: rune.arnesen@jotne.com)


Q:
Which is the equivalent material P255QL EN 10216-4 in DIN standards?
(asked by: inamarro@yahoo.com)

A:
P255QL is W.Nr. (Werkstoffnummer) in DIN standard!
See also Mannesmann Präzisrohr: http://www.mhptubes.de/3340-psrfakw.htm


Q:
What is the difference between DIN EN and DIN, for example DIN EN 10305-1 and DIN 2391?
(asked by: yong.wang@benteler.de)

A:
AFNOR, B.S., DIN, SS, UNE, UNI etc. are national standards from particular members of European Union which are integrated and renumbered in the common EN (European Norms).


Q:
What material is Ac 37-2 DIN 17100 and what is its alloy composition?
(asked by: nitesh.kalra@in.transport.bombardier.com)

A:
In Stahlschlüssel (German: Steel key) there is no Ac 37-2! There is only Ac-1, identical with St 37-2, with the following chemical composition:
C max. = 0.20%, P max. = 0.07%, S max. = 0.05%.
It is unalloyed and bright general structural steel.


Q:
I am designing a gas pipeline as per ASME B31.8. The specification calls for API 5L Gr B materials pipes. Can I replace this pipe material with ASTM A106 Gr B which is readily available in local market? Please give technical justifications. Thanks!

A:
Each supplier of mentioned materials can provide you with their chemical & mechanical properties, their equivalents and purposes.
As the designer (an expert) of particular pipeline project, only you must overtake decision and responsibility which material to apply!
Nobody else will do it instead of you!
As an expert in this field you have sure some specialized institutions that you can consult, but last decision will be always yours.

(asked by: johnbritto@knm-group.com)


Q:
What is the ASTM equivalent for DIN St 45.8/III steel?
(asked by: icerizola@fanapel.com.uy)

A:
A 106 Grade B


Q:
Could you tell me the conductivity factor (W/mK) for STB 340?
(asked by: bob@sunssteel.com)

A:
JIS G3461 Carbon Steel Tubes for Boiler and Heat Exchanger (JIS G 3461/JISG3461)
Class Symbols (Applicable till the end of 1990): These tubes are classified into 3 grades and their class symbols are given as:
Class new/Traditional symbol (Informative reference)
STB 340/STB 35
STB 410/STB 42
STB 510/STB 52

Therefore this question ask at:
Japanese Standards Association
Web site: http://www.jsa.or.jp/default_english.asp
Email: sitemaster@jsa.or.jp


Q:
We need to know how we can get Hydrant, Pipes & Sprinkler? The Manufacturer, their address, telephone. Thanks.
(asked by: jkn@linkserve.com)

A:
Become a member of this web site and post for free your inquiry ad.


Q:
What is the DIN standard equivalent to material SA213 T22?
(asked by: r_sekar@aprilasia.com)

A:
ASTM/ASME = A213 T22/SA199 T22 ≈ DIN = 17175/10CrMo910 ≈ BS = 3606 622 ≈ ISO = 2604 II TS34 ≈ JIS G 3462 = STBA 24
Source: http://www.jfe-steel.co.jp/en/products/pipes/speciality/comparison.html


Q:
What is the ASTM comparable for SAE 8620?
(asked by: wricomntg@wrico-net.com)

A:
AISI/SAE/ASTM 8620 ≈ DIN 21 NiCrMo 2 = W.Nr. 1.6523 ≈ AFNOR 20 NCD 2 ≈ B.S. 805 B 20 ≈ UNI 20 NiCrMo 2 ≈ JIS SNCM 220 (H) ≈ SS 2506 ≈ UNE F.1522 - 20 NiCrMo 2; F.1534 - 20 NiCrMo 31


Q:
What is the equivalent for ST37, DIN-1626 in ASTM standards?
(asked by: vsgvprasadarao@yahoo.co.in)

A:
See answer given to walterkowalski@Univsteel.com


Q:
Please tell me Material compositions of GB 8162 Grade & ST35/ST37.5/DIN1629
(asked by: hymaplates@yahoo.com)

A:
GB 8162-82 YB(T)63-87: C = 0.42-0.50%, Si = 0.17-0.37%, Mn = 0.50-0.80%, P = 0.035%, S = 0.035%, Ni = 0.25%, Cr=0.25%, Cu0.25% (source: www.saleroad.com/know/steel/1011.htm)
St 35-3: C max. = 0,16%, Mn = 0,35 - 0,65%, P max. = 0,040%, S max. = 0,040%, Cr max. = 0,30%, Ni max. = 0,30%, Al max. = 0,02%, Cu max. = 0,30%, Cr + Cu + Ni max. = 0,70%
St 37-2 % max.: C = 0,17%, P = 0,050%, S = 0,050%, N = 0,009% (St 37.5 doesn't exist)


Q:
What tube material is equivalent to E 235? And is it readily available in India
(asked by: ramasteelforge@yahoo.com)

A:
I don't know the meaning of E 235!


Q:
Can I replace steel Rst 37-2 by AISI304? Thank you!
(asked by: rasa@accel.lt)

A:
RSt 37-2, W.Nr. 1.0038 is equivalent to AISI/SAE/ASTM A 570 Gr. 36. Whether you can replace it with AISI 304 you must ask a designer or an expert of the particular project where you want to apply it.


Q:
1) What is difference between German steel designation St 50 and St 50-2.
2) What whould be the closest US equivalent for both?
(asked by: Don.Kuhns@alcoa.com)

A:
1) St 50 (max %): C = 0.32, P = 0.080, S = 0.060
St 50-2: C = 0.28 - 0.37, Si = 0.17 - 0.37, Mn = 0.50 - 0.80, P = 0.045, S = 0.050, Cr = 0.30, Ni = 0.30, Cu = 0.30
2) For both see answer to bobl@centacorp.com


Q:
What is the composition for 34CrMo4?
(asked by: carole.tan@jenmon.com)

A:
DIN 34 CrMo 4 = W.Nr. 1.7220 (% max.): C=0.30-0.37, Si=0.15-0.40, Mn=0.50-0.80, P=0.035, S=0.035, Cr=0.90-1.20, Mo=0.15-0.30


Q:
Which is the equivalent material in DIN of DC04 and DC05?
(asked by: andrzej.liszka@multimet.com.pl)

A:
Ternex is manufactured to British Standard BS 6582 :1985. The steel substrate is to EN 10130 : 1999 in the following grades: DC01, DC03, DC04, DC05, DC06.
Continuously hot-dip lead alloy coated cold rolled carbon and austenitic stainless steel flat rolled products.
It is not related to any other standard.


Q: What is the equivalent material of DIN 1654 Part 4 19MnB4 in JIS or in Chinees (GB) Material standard?
(asked by: hsarman@seger.com & demeric@veezy.com)

A:
DIN 19MNB4 = EN 22MNB4 = AFNOR 20MB5 = AISI 10B21 = JIS SWRCH22A = UNI C23BKB
GB = I don't know!


Q:
What is the material specification, chemical composition and equivelant material of A 204 Gr B plate material?
(asked by: sureshthaker2002@yahoo.com)

A:
Find it out at http://www.stalforbund.com/Fagomraader/Materialer/steel_carbon.htm


Q:
What is the ASME equivalent and "P" No. grouping for DIN 2391 st 52?
(asked by: pravin.laljit@murrob.com & Nathanael.Govender@murrob.com)

A:
DIN 2391 is German standard for seamless precision steel tubes.
For St 52 see previous question asked by iranweld@yahoo.com


Q:
What are the BS equivalents to ASTM A53GrA and B (or old EN)?
(asked by: terence.sundgren@eskom.co.za)

A:
BS 1387


Q:
What is the specification/dimensional size of ISO 2852, 1 1/2" Tri-Clamp?
(asked by: bahrin_shah@westpharma.com)

A:
See it at www.google.com with the following search string: Tri-Clamp ISO 2852


Q:
What is the meaning of MS ST35/ST37.5/DIN1629?
(asked by: hymaplates@yahoo.com)

A:
MS = Mild Steel. Also as Mannesmann's method of tubes production (seamless) – more frequent in such connotation
St 35, St 37 = Steel Qualities (St 37.5 doesn't exist)
DIN 1629 = Technical conditions of supply


Q:
What steel can be used to substitute EN16T?
(asked by: rcarvalho@tstt.net.tt)

A:
Steel EN16T is similar to BS 970: 1983 606M36T, Hitenspeed 55T.


Q:
How to prevent the crack formation during hot rolling of duplex stainless steel grade Din 1.4462?
(asked by: bariar@facorsteel.com)

A:
Generally, such questions cannot be answered by web master of this web site.
Suggestion: go to www.google.com and write search phrases like the following one: crack formation during hot rolling


Q:
What is the alloy composition of API 5 CT?
(asked by: m.szymczewski@wp.pl)

A:
Find it at: http://www.arvedi.it/ata/api1.htm or http://www.jindal.com/seam-product.htm etc.


Q:
What is DIN St 52-3 and does it relate to any ASTM specifications?
(asked by: iranweld@yahoo.com)

A:
St 52-3 = W.Nr.1.0570 is the carbon steel with the following composition:
C ≤ 0.20%, Si ≤ 0.55%, Mn ≤ 1.60%, P ≤ 0.040%, S ≤ 0.040%.
Its equivalents are:
AFNOR - E 36-3; E-36-4, B.S. - 4360-50 B; 50 C; 50 D, UNI - Fe 510 B; C; D, JIS - SM 50 YB; SM 53 B; C, SS - 2132, GOST - 17 GS; 17 G 1 S, UNE - A 510 C; D; F. 6214 AE 355-C, AISI/SAE/ASTM - A 572 Gr. 50; 1024; 1524; K 12709.
See also other equivalents at: http://www.steeltubestrade.net/tech_standards.php


Q:
What is DIN St 37.2 and does it relate to any ASTM specifications?
(asked by: walterkowalski@Univsteel.com)

A:
It is carbon steel, W.Nr. 1.0037, DIN St 37-2 with the following composition (the same as RSt 37-2): C ≤ 0.17%, P ≤ 0.050%, S ≤ 0.050%, N ≤ 0.009%. It doesn't relate to any ASTM, but there are two other similar which do:

W.Nr. 1.0036, DIN USt 37-2 (Germany) = AFNOR E 24-2 (France) = B.S. 4360 B (Great Britain) = UNI Fe 360 B Fu (Italy) = JIS SS34 (Japan) = SS 1312; 1311 (Sweden) = GOST 16 D; 18 kp (Russia) = UNE A 360 B; F.6202-AE 235-B (Spain) = AISI/SAE/ASTM A 570 Gr. 33, 36 (U.S.A.)

W.Nr. 1.0038, DIN RSt 37-2 = AFNOR E 24-2 NE = B.S. 4360-40 C = UNI Fe 360 B FN = JIS SS 34 = SS 1312 = GOST BSt 3 sp 2 = UNE - = AISI/SAE/ASTM A 570 Gr. 36


Q:
SA 516 GR 70 MTLTV - what does MTLTV Stands for?
(asked by: amirah@igawara.com.sg)

A:
It has not any meaning in connection to this steel for pressure vessel


Q:
What are the ASTM equivalents for DIN EN 10204-3.1, DIN 1623, DIN 10203, DIN 50049, DIN 10088, DIN 60672?
(asked by: wmoore@airinterus.com)

A:
DIN EN 10204-3.1 = ASTM A105, DIN-1623 St 12.03 = ASTM A568/366, EN 10203 = ASTM A 625 -92, DIN 50049 = certification standards, EN 10088 = ASTM A312/312M, IEC 60672-3:1997 = DIN EN 60672-3 = ISO12986-2:2005 = ASTM C 651:1991


Q:
What is the Chinese equivalent or most close material to SAE-4130? Thanks.
(asked by: aradf@barak.net.il)

A:
I don't know it. If anybody knows it please help!


Q:
Could you provide the chemical composition of GOST 8732-78/8731-74 and what is the ASTM equivalent?
(asked by: bob@sunssteel.com)

A:
Seamless Pipes in CIS are produced as for sizes acc to:
GOST 8731 & 8732 as Hot Rolled Seamless Pipes
GOST 8733 & 8734 as Cold Drawn Seamless Pipes
However, as for steel grades are mostly used GOST 1050-88
The main grades are 10, 15, 20, 35, 40 and 45.
Gr. "20" acc. to GOST 1050 is equivalent to Gr. "B" acc. to ASTM A 106/A53..
For Casing and/or Tubing pipes sometimes grade is not indicated at all and indicated only a letter as "K", "D" etc. acc. to related yield and tensile strengths.
The same in API standard designated for Oil & Gas Industry mostly used Grades as "B", X42 X52 etc.
Also other grades applicable acc. to relevant standards DIN, EN, ASTM.

See also this link: http://www.dts.dp.ua/info/gost/pipes/index.php


Q:
What is US equivalent to ST 50-2 steel grade?
(asked by: bobl@centacorp.com)

A:
General structural steel
DIN (German) Standard St 50-2 = W.Nr. 1.0050 = NS 13234 (Norwegian) Standard.
There are no other equivalents.


Q:
What is ST. 52 steel? Is this a Eurpoean standard?
(asked by: dmiller@viasystems.com)

A:
It is German Standard (DIN Standard).


Q:
EN 10305 equivalent material in astm standard?
(asked by: ravi.kolur@chemtexblr.co.in)

A:
See previously answered questions to gundars_erdmanis@ssl.lv and onkarnath@sprayindia.com


Q:
What is the tensile strength of 1/4" wall 1.5" x 2.5" aluminum rectangular tube?
(asked by: matthewf@custombuildingsystems.net)

A:
I don't know. If anybody knows it, please help!


Q:
What is the difference between ASTM X 42 and Gr. B?
(asked by: bob@sunssteel.com)

A:
Steel for large diameter pipes
Material No = according to EN 10208-2 = DIN 17172 = API 5L
1.0457 = L 245NB = StE 240.7 = Gr. B
1.0484 = L 290NB = StE 290.7 = X 42

Source: http://www.stalforbund.com/Fagomraader/Materialer/steel_carbon_2.htm


Q:
What do the following abbreviations in DIN 1629 (k; bk; bkw; gbk; nbk) mean?
(asked by: aasynch@online.ru)

A:
k = I don't know, bk = cold finished (hard), bkw = cold finished (soft), gbk = annealed, nbk = normalized - acc. DIN 2391.


Q:
Where can I get DIN 1629 in English?
(asked by: aasynch@online.ru)

A:
Find it out through e-pipe Korea at: http://www.e-pipe.co.kr/cgi-bin/search_text_new_eng.cgi?keyword=DIN%201629

More complete overview you can get also at: http://answers.google.com/answers/threadview?id=59674


Q:
Can forging of Din 2391 - ST 52 be possible? I want to know whether yield strength of this material is 525 N/sq.mm?
(asked by: sumashiva03@yahoo.com)

A:
It could be possible but is not usual except for cylinder tubes (inside diameter). Yield strength of St 52 is 490 - 630 N/sq. mm


Q:
What is the chemical composition of ST 37.2 steel?
(asked by: ginforge_manish@hotmail.com)

A:
See previous question!


Q:
Please provide chemical composition for St 37.2 and St 50
(asked by: ginforge@jla.vsnl.net.in)

A:
St 37-2, DIN Standard 12120, W.Nr. 1.0037: C ≤ 0,17%, P ≤ 0,050%, S ≤ 0,050%, Others: N ≤ 0,009%

St 50, DIN Standard 7960: C ~ 0,32%, P ≤ 0,080%, S ≤ 0,060%


Q:
What is ASTM equivalent of material DIN 1.4462?
(asked by: sushil_jaggi@lurgi.de)

A:
Standards - Sandvik Grade: SANMAC SAF 2205, ASTM: S31803, EN: 1.4462*, W Nr.: 1.4462, DIN: X 2 CrNiMoN 22 5 3, SS: 2377
Product standards Bars and shapes: ASTM A479, EN 10088-3*, ASTM A276, Billets: EN 10088-3*, SEW 400.
Chemical composition (nominal) % = C max = 0.030, Si max = 1.0, Mn max = 2.0, P max = 0.030, S max = 0.015, Cr = 22, Ni = 5.5, Mo = 3.2, N = 0.18
Certificate: Status according to EN 10204/3.1.B
Forms of supply: Bar and billet
Billets, round as well as round-cornered square, are produced in sizes 80 – 350 mm.
Round bar is supplied in the solution annealed and quenched and peel-turned condition. The principal size range is 20 – 350 mm.
Other products: Cast products; Covered electrodes; Fittings and flanges; Forged products; Plate, sheet and wide strip; Seamless tube and pipe; Strip electrodes and flux for surfacing; Strip, annealed or cold-rolled to different degrees of hardness; Welded tube and pipe; Wire electrodes and filler wire/rods

* According to EN 10088, valid for sheet/plate, strip, semi-finished products, bars, rods and sections for general purposes.

(Source: Sandvik)


Q:
What is the standard working pressure for BS 1387 black and galvanized pipes?
(asked by: hsiakk@tm.net.my)

A:
Up to 219.1 mm od = 64 bar max.
Over 219.1 to 660 mm = 25 bar max.
Over 660 mm = 16 bar max.


Q:
a) St 37.8/I tubes what is the composition and type?.
b) What is the difference between 16Mo3 and 15Mo3 steel?
(asked by: han_acharya@yahoo.com)

A:
a) Find it at: http://www.mertl.com/englisch/downloads_e.htm
b) There is no difference. DIN 17175 = 15 Mo 3, EN 10216-2 = 16 Mo 3.


Q:
Does anyone know the NEN and ISO norm for AISI 4130?
(asked by: revon@wxs.nl)

A:
AISI 4130 ~ 25CrMo4 = 1.7218/34CrMo4 = 1.7220 is low-alloy steel for onshore/offshore gas/oil components.
Composition of heat–treatable low–alloy steel and pipe for petrochemical components for use in non-sour or sour environment is: C = 0.28-0.33%, Si = 0.15-0.35%, Mn = 0.40-0.60%, Cr = 0.80-1.10%, Mo = 0.15-0.25%


Q:
What is a ANSI/ASME/API/ASTM equivalent to ST-53.3 steel?
(asked by: gwoods@technip.com)

A:
Steel St 53-3 doesn't exist


Q:
Which GTAW (or FCAW) consumable should I use to weld 15 Mo 3 and 16 Mo 3 steels?
(asked by: regis@labsolda.ufsc.br)

A:
Ask this question at:
Böhler Thyssen Schweißtechnik GmbH
Hansaallee 321
Gebäude/Building 30
D-40549 Düsseldorf
tel +49 (0)211 580 660-0
fax +49 (0)211 580 660-12
mail: info@boehler-thyssen.com
web: http://www.boehler-thyssen.com/


Q: We have some heat exchanger tubes identified in drawing as SA-179 Killed. I checked ASME SA-179. It does not specify any killed or non-killed material. Please confirm is there any SA-179 tube with killed grading?
(asked by: khansh@petrokemya.sabic.com)

A:
SA 179 is not killed steel but it can be ordered as killed with minimum Al content of 0.02%. Similar steel is SAE 1010.


Q:
Which EN standard is previous E235?
(asked by: gundars_erdmanis@ssl.lv)

A:
EN 10305 - Steel name E355 = DIN 2391 - St. 52 = UNI 7954:79 - Fe 490
Steel tubes for precision applications.


Q:
Which is the Equivalent material in AISI of 25CrMoS4?
(asked by: umapathy@indimet.com)

A:
DIN 25CrMoS4 = W.Nr. 1.7213 = ISO 25CrMoS4 = AFNOR 25CD4u


Q:
What is the exact equivalent of Q235B in DIN standards?
(asked by: ozcanmustafa75@hotmail.com)

A:
Find it at: http://www.ssec-steel.com/tool/tool3-2.html


Q:
Please provide me tensile strength and yield strength of API 5L GR B.
(asked by: immmrann@yahoo.com)

A:
Minimum yield strength = 241 Mpa.
Minimum ultimate tensile strength = 413 Mpa.


Q:
Where can I find the nearly similar/equal steel material comparison chart for various standards and codes?
(asked by: mjindalin@advanceafro.com)

A:
Some of them you can find at this web site under Technical data.
Otherwise search them over www.google.com by using the similar strings like: ASTM Standards, BS Standards, DIN Standards, JIS Standards etc.


Q:
What is the definition of DIN 1629 ST 52 HFS example what does the ST stand for?
(asked by: m.gaskin@ladbrookuk.com)

A:
St stands for German Stahl (English Steel).
Detailed answer please find at: http://www.europeantubes.co.uk/hfs.htm


Q:
Dear sir, can you send Chemical composition, Mechanical properties of material, Producing pursuant to the standard, etc. of carbon welded steel pipes, steel grade q 195 - q 215 (Chinese standard)?
(asked by: alfaniah@emirates.net.ae)

A:
Find it over Useful links at: e-pipe Co., Ltd.


Q: a) Seamless pipe availability in material 15Mo3 (DIN17175 & DIN2448 )& suitability of same for steam service at max temperature 463 C?
b) ASTM equivalent & Pipe grade for the same?
c) Any constrains for welding valve with WC9 body to 15Mo3?

A:
a) See previous question asked by: phantomlord_met@yahoo.com!
b) See previous question asked by: gary@camelotconsolidated.com!
c) See previous question asked by: phantomlord_met@yahoo.com!


(asked by: balachandran_t@jalal.com)


Q:
May I replace A53 Gr B. instead of DIN 2448 for Fire fighting pipeline?
(asked by: phantomlord_met@yahoo.com)

A:
All such and similar decisions may be only made by responsible expert engineer of the respective plant!


Q:
How can i get the basic data for selection of gear boxes in ROTARY KILNS?
(asked by: avijit_avijit@yahoo.com)

A:
Search "ROTARY KILNS" over www.google.com


Q:
Where can i get mechanical properties of St 45.8?
(asked by: nunofsdias@gmail.com)

A:
You can get it at:
http://www.sinara.de/sin17175_e.html
http://www.trubky.cz/engl/mechprop.htm


Q:
What is the equivalent EN of ST 35?
(asked by: sdsarkar@flenderindia.com)

A:
DIN St 35 = W. Nr. 1.0308 = EN E 235


Q:
What is the DIN or British standard equivalent to ASTM 53 GRADE B for raising pipe?
(asked by: hfayez@nets.com.jo)

A:
Welded water & gas pipes are produced as light, medium and heavy series according to: ASTM A-53, BS 1387, DIN 2440 - DIN 2441, ISO 65, NFA 49-145, UNI 8863.


Q:
What is the tensile strength of ST 37.2
(asked by: pelaez_ray@yahoo.com)

A:
Material - St 37.2
Material No - 1.0038
Tensile strength, Rm, N/mm² - 340.0 - 470.0
Yield strength, min., Ren, N/mm² - 235.0
Elongation, min., A5, per cent - 26.0

Material - St 44.2
Material No - 1.0044
Tensile strength, Rm, N/mm² - 410.0 - 540.0
Yield strength, min., Ren, N/mm² - 275.0
Elongation, min., A5, per cent - 22.0

Material - St 52.3
Material No - 1.0570
Tensile strength, Rm, N/mm² - 490.0 - 630.0
Yield strength, min., Ren, N/mm² - 355.0
Elongation, min., A5, per cent - 22.0


Q:
What is American equivalent to 16M03 material?
(asked by: gary@camelotconsolidated.com)

A:
DIN 16 Mo 3 - W. Nr. 1.5415 = AISI/SAE/ASTM - A 204 Gr. A


Q:
What is the replacement or Equivalent of DIN 2391/C carbon steel tube?
(asked by: ambanimetal@vsnl.net)

A:
All seamless precision steel tubes used as pressure lines for hydraulic and pneumatic purposes. Search over www.google.com equivalents for DIN 2445/2, EN 10204.


Q:
Can I use stainless 440C as replacement for the following materials; UNI 7847 and ASTM-A193?
(asked by: globalsphere@gmail.com)

A:
The same as the previous one. If anybody knows it, please help!
Ratko


Q:
What is the replacement materials type for UNI7847 and ASTM A193?
(asked by: globalsphere@gmail.com)

A:
I don't know it. If anybody knows it, please help!
Ratko Balosic


Q:
What is the equivalent DIN Number of ASTM A53 Gr B?
(asked by: quasiy@yahoo.com)

A:
ASTM A 53/ASME SA 53 - Seamless and welded (ERW) carbon (black) steel pipes = DIN 1626 St 37.2, DIN 1629 St 35, DIN 1629 St 45, DIN 1626 St 42-2


Q:
What is the XXX S in Pipes?
(asked by: amardeepsteel@yahoo.com)

A:
See at: http://www.bivar.com/pdf/02opto15.pdf


Q:
What is the DIN equivalent of SA 178 and SA 179?
(asked by: viratradelinks@hathway.com)

A:
Boiler tubes

ASTM/ASME A/SA-178 = Grades A and C. Electric Resistance Welded Carbon Steel Boiler Tubes = DIN 17177, Steel 37.8 I - III, Steel 42.8 I - III

ASTM/ASME A/SA-179 = Seamless Cold-Drawn low-Carbon Steel Heat Exchanger and Condenser Tubes = DIN 17175, Steel St 35.8, St 45.8, 15Mo3, 13CrMo44, 10CrMo910


Q:
What is the equivalent material of DIN 2448 in ASTM
(asked by: onkarnath@sprayindia.com)

A:
1. Cold Drawn and/or Hot Rolled Boiler and Heat Exchange Pipes, according to: DIN 2448, DIN 2491, DIN 8180, DIN 17175, ASTM A179, ASTM A106, ASTM A210, ASTM A192, ASTM A193, ASTM A209, ASTM A213, GOST 8733, GOST 8734
Steel Grade: A, B - acc. to ASTM
ST 35.8, ST 45.8, 15Mo3, 13CrMo44 - acc. to DIN
Dimensions: Outside diameter 8 - 168.3 mm
Wall Thickness: 1 - 22 mm

2. Lines Pipes, acording to: API 5L, DIN 2448, GOST 8731, GOST 8732
Steel Grade: A, B, X42, X46, X52, X56 - acc. to ASTM
ST 35 - acc. to DIN
Dimensions: Outside diameter 3/8 - 6.5/8 in (17.1 - 168.3 mm)
Wall Thickness: 0.091 - 0.625 in (2.31 - 15.9 mm)

3. Structural Pipes, according to: DIN 1629, DIN 1630, DIN 2391, DIN 2448, ASTM A53, ASTM A501, ASTM A501, ASTMA 106, GOST 8731, GOST 8732
Steel Grade: A, B - acc. to ASTM
ST. 37, ST 37.4, ST 44.4, ST 52, ST 52.4 - acc. to DIN
Dimensions: Outside diameter: 8 - 168 mm
Wall Thickness: 1.00 - 22 mm


Q:
Where can I find Material Test Reports in your website?
(asked by: lyndie_knockleby@kineticprocess.ab.ca)

A:
You will find them through Useful links (e-pipe.co.kr, iransteelcenter.com, mesteel.com, tubenet.org etc.)


Q:
What is equivalent of 25CrMo4V to ASTM/AISI?
(asked by: pandithan_kg@perkasa.co.id)

A:
DIN 25CrMo4 = W.Nr. 1.7218
W.Nr. 1.7218 = AISI/SAE/ASTM 4130


Q:
I am looking for a distributor for steel seamless tube called "mecaval 147 mk"
(asked by: woodman.drw@on.aibn.com)

A:
As an Exclusive member you can find 6 different suppliers for the required tubes, from those who have joined the products to their account, under following products:
13518 – Micropiles
13799 - Tubes for foundation piles
13801 - Tubes for foundations


Q:
I am seeing steel pricing designated by currency (eg. USD), weight (eg. MT), and with CIF, what does CIF mean?
(asked by: szetu@rogers.com)

A:
Find it under Technical Data/Incoterms.


Q:
What is the meaning of V In the steel 25CrMo4V?
(asked by: manhajialigol@yahoo.com)

A:
Vanadium


Q:
How can I get to know all inquiries for aluminum tubes and pipes?
(asked by: eastcorp123@vsnl.net)

A:
Dear Mr. Anant Shri Kajaria,
This is a very good question!
There are two ways:

1) As a FM (free member) you can request basic data of all companies, which have posted inquiry or offer ads. You will get them for free, chronologically ordered (by dates), in an Excel table with an empty Manipulation Column (MC). Go through posted ads and mark interested ads in MC as e.g. Al-P (P = purchase). Sort then your Excel according MC, hide un-necessary columns and copy & paste interesting data in a Notepad and from it in your working database. As a FM you can also see in the Special directory how many companies, which have jointed their products, buy and sell Al - pipes.

2) As an EM (exclusive member) you'll get automatically basic data with short program description of all companies currently added in the Special directory and its monthly updates. Go to the Special directory, click at Products and then at Group 21000. Find interested Al - pipes. You can click at product's code to get them all or at suppliers or purchasers. You'll get the relating companies in an alphabetical order. In your MC you can mark them as Al-P (purchaser) or Al-S (supplier). There are much more companies in Sd without jointed products. To include also them in your working database, sort your Excel according short description and make then fine research in Program description from the interesting companies using this web site.


Q:
Could you please tell me the main mechanical tests required and chemical analysis of material (aluminium coated) which fit ASTM A463?
(asked by: choupipe@hotmail.com)

A:
You'll find it through E-Pipe Co, Iransteelcenter, Mesteel, Maryland Metrics etc. given in the Useful links.


Q:
What is the meaning of FAQs?
(asked by: mouna@sabouni-group.com)

A:
Frequently Asked Questions


Q:
I want know some stocks and supplier for purchase welded and seamless steel pipe according DIN 2448 AND 2458 in uae country. Can you help me?
(asked by: pureng.shipbld@isoico.com)

A:
At your request, as a qualified free member* you can get currently updated Public directory and as an exclusive member currently updated Special directory and its monthly updates.
These services are new and free of charge.
Qualified member* = who completed the form "My company's data".


Q:
What is the mean of "SCH"?
(asked by: chishan@besttube.net)

A:
Schedule in ANSI/ASTM Standards.


Q:
DOT cylinders. What it means "DOT"?
(asked by: prasad@esisaws.com)

A:
I don't know. If anybody knows it, please help!
---------------------------------------------------
Subject: Got Answer for my question
Dear Ratko Balosic,
Your website is simply the best.
For my previous question, DOT cylinders. What is "DOT"?
I got the answer and i am sending for your information.
Cylinders which are made according to DOT Specifications are called DOT cylinders.
DOT - Department of Transportation, USA.
Thanks & Regards
N.V.S.PRASAD


Q:
Sir, I want to edit my inquiry, my company details and save them again. How?
(asked by: prasad@esisaws.com)

A:
For editing all your ads follow step-by-step Instructions given under Home link.
For deleting a company's ad or a membership's ad contact us.


Q:
Tube length = 10"NB. What does it mean NB?
(asked by: prasad@esisaws.com)

A:
Deutsch (German): Normalisiert Blank
English: bright thermal stress relief (normalized bright).


Q:
What means "hfn" added after mark of steel?
(asked by: silvia_mitova@hotmail.com)

A:
Hot formed (forged, rolled), normalized.
Ms. Mitova - advised through a Dutch friend.


Q:
What does C&F mean?
(asked by: ariunsanaa@newcom.mn)

A:
Nothing! See Technical data/Incoterms/CFR - explanation.


Q:
What is the difference between Tube and Pipe?
(asked by: ingrole@pcoc-adityabirla.com)

A:
In tube & pipe industry there is no difference with an exception - pipes in all their meanings are always inside round. In English both words have several different meanings. See also in Useful links http://www.onelook.com/browse.shtml - Browse Dictionaries


Q:
Where can I get extensive information about chinese steel or a list of chinese steel (compounds) or a list that assigns chinese steel to other standards (best case: german ones)?
(asked by: wolfgang.schricker@de.bosch.com)

A:
Try it through:
Ms. Susan, susan@yieh.com, http://www.yieh.com
http://www.tdctrade.com:
http://www.hktrader.net/200402/index/index20040203.htm:
http://www.klako.com/en/cf/c.html


Q:
How do I post an enquiry for buying? Please advise.
(asked by: valtec@lycos.co.uk)

A:
Log in as the member, click at MEMBER'S AREA, then at Inquiries and finally at Add new inquiry. Complete the form and click at Save changes.
Your ad is already published.


Q:
What is the difference between st 37 and rst 37?
(asked by: sab@ssn.co.ir)

A:
St 37 - Way of deoxydation: -; Condition: U = untreated and N=Normalized
RSt 37 - Way of deoxydation: R=killed; Condition: U=untreated and N=Normalized
RRSt 37 - Way of deoxydation: RR=specially killed; Condition: U=untreated (longitudinal) and N=Normalized (transvers)
USt 37 - Way of deoxydation: U=rimmed; Condition: U=untreated and N=Normalized


Q:
Will you be kind and provide me few addresses of Russian and Ukrainian grossest which sell seamless pipes, please.
(asked by: ferumva@ptt.yu)

A:
You can find them yourself in the Public and Special directory and save them in your PC or print them out.


Q:
I HAVE BECOME A FREE MEMBER, HOW CAN I ADD MY INQUIRY?
(asked by: wsy@lubaosteeltube.com)

A:
By following step-by-step Instructions given under Home link.


Q:
I have registerd my company details but still not become free member and can not surf.
(asked by: uicindia@hotmail.com)

A:
Please log in, click at MEMBER'S AREA and then go to My company data. Fill up your basic company data and click at Save changes (just follow Instructions given under Home link).


Q:
How can I post my message?
(asked by: sales@china-shangang.com)

A:
You have to become our full Free member (with your company's data). Do it first and then just follow Instructions given under Home link.


Q:
Can I add the same inquiry (offer) at a continental and the global level?

A:
Yes, you can.


Q:
How many inquiries (offers) can I place at your site?

A:
There are no limits.


Source:  www.steeltrade.net

 

(c)2000,2004 SteelTubesTrade.net  

 

Comments

amin said…
Hi Sir, I want to know what is welding metallurgy of sa516 grade60, and does this material is heat treated? how to identify and know what is mean by SA516 Gr60, and in AISI standard,, what is the code using same material as SA516 gr60

Please Help mE!!!!
Anonymous said…
Hi Sir,
I need to know about heat treatment of this type of steel, "API 5CT L80, Type1"?
how we can get high impact energy & Yeild stress vs low hardness?
Thanks
Mr Amin
SA 516 Gr 60 is plate material, generallu used for construction of process equipment, It is an ASME stanadrad (refer ASME BPV code SecIIA for more details under SA516), it this can be normalised or Q&T, N&T depending on your rquirement

Raghuram
Anonymous said…
Elmar Sultanov (sales@ktbits.com)

what is the equivalent ST52 to GOST - russian standard... i know some sites shows 17 GS but we can't find the right one..

also i am intersted in component of ST52 material

thanks
St52 is a structural steel material with 0.2% C, 0.04% S$P, UTS 510-680, YS355 N/mm2
Anonymous said…
HI I WANTED TO KNOW WHAT IS equivalent DIN number of API 5CT l80 TYPE1?
THANKS FOR YOUR GUIDANCE
Anonymous said…
Hi Sir,
I need to know about heat treatment of this type of steel, "API 5CT L80, Type1"?
how we can get high impact energy & Yeild stress vs low hardness?
Thanks
Anonymous said…
I want to have a ST44-2 modulus of elasticity(E)
Anonymous said…
1) I want to conduct Welder qualification test API 5L X56, what is equivalent material in ASME? Due to non availability of Actual material

2) I want to conduct Welder qualification for BS EN 10025 Part 3 S355 NL material, what is equivalent material in ASME? Due to non availability of Actual material

Skumarswami@yahoo.co.in
Anonymous said…
1) I want to conduct Welder qualification test API 5L X56, what is equivalent material in ASME? Due to non availability of Actual material

2) I want to conduct Welder qualification for BS EN 10025 Part 3 S355 NL material, what is equivalent material in ASME? Due to non availability of Actual material

Skumarswami@yahoo.co.in
Dear all please send your querries to "materials-welding@googlegroups.com" for quci reply
To subscribe this group, send email to materials-welding-subscribe@googlegroups.com
Anonymous said…
you have a wonderful site!
Unknown said…
Hello everyone,

I am buying materials for a water impulsion that was designed following AWWA c200. My question is related with the elbows because they were specified to be API 5L GrB, AWWA C208, and diameter 48in.

The vendor is quoting the elbow AWWA C208, but ASTM A36.

I would like to have some advise to make the right decision.

Thanks
Unknown said…
Hello every body, I am the newer here. Could you please tell me: GOST 8731-74/8732-78 are equivalent to wht API?
Unknown said…
Hi sir, may i know what is the thermal conductivity for the ASTM A 213/T22? or is there any websites provide the thermal conductivity for carbon steel tube?
thanks.
Unknown said…
hi what is the indian standard for astm a-36 material? which material should i buy
Unknown said…
Sir,
Pls say what is the Chemical Composition for MS Billet grade ASTM 510
SAE 1524

Pls know email scintilla_bd@yahoo.com
Unknown said…
Sir,
Pls say what is the Chemical Composition for MS Billet grade ASTM 510 &
SAE 1524

Pls know email scintilla_bd@yahoo.com
Anonymous said…
hello,
i need suppliers from europe for 15Mo3, 16Mo3, S.S310.
My e-mail: jame.mech@yahoo.com
Anonymous said…
Hello Sir,

Where can i find a formulae in computing the ultimate strength..
..or if you know that value for SNCM220..Thanks,
Anonymous said…
Sir,

Do you know where i can find a formulae for calculating ultimate strength for SNCM220..
or if you knew the values..
thank you,

regards,
venice

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...