Skip to main content

Re: [MW:35853] Welding of dissimilar metals

Hi Mulenga,

I currently have such a calculation. I used it in my previous works. There are 3 alternatives for you. It can be used as an alloy and transition wire. Don't forget to check your own calculations and the FN region. The De Long diagram is good.

  1. ErNiCr3 SFA A5.14 >> Since the Cr Ni ratio will be high, the Ferrite ratio in Duplex should not fall below 30%.
  2. Duplex ER2209 SFA A.9 >>> Seems ideal. Since there will be a combination of 304 different materials, there will be some loss of chemical properties of the superduplex. In fact, you get a complete Duplex.
  3. Superduplex ER2594 SFA A5.9 >>> Definitely the best. The amount of Cr in the weld metal will increase. The amount of Ni also to a very small extent. In both options, you remain in the Austenite+Ferrite region. Don't forget to do a cost calculation according to the importance of the job. <<<

Maybe I don't need to say it, but use 100% Ar as Shielding and Backing gas. If you have the opportunity, 2.5% Nitrogen for Backing can prevent root darkening. This also provides better corrosion resistance. O2 max 250 ppm !!
You should keep the heat input to a minimum, use values as low as you can. (interpass should be max 50°) All these are information that will definitely work for you for butt welds. Good work.


21 Ekim 2025 Salı tarihinde saat 09:43:03 UTC+3 itibarıyla Rilley Chellah Mulenga şunları yazdı:
The duplex steel grade is  SAF 2507

On Mon, 20 Oct 2025 at 17:51, Vishwas Keskar <vvkes...@gmail.com> wrote:
What is the 108 duplex steel ?

Pl inform Duplex garde?


On Mon, 20 Oct 2025 at 9:12 PM, Rilley Chellah Mulenga <rilley....@ahkgroup.com> wrote:
Good day experts ,

we encountered  a challenge trying to reducers of 108 duplex steel to mild steel and welding 108 duplex stainless steel steel to 304 stainless schedule 80, what is the best filler rods i can use when using TIG 

--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHkXHT-Hsg%3DXK%2BVVkODpOBUYA%2BBHAD5t%3DdQwwa5rOAQWDADfFQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


--
Thanks & kind regards


EmailLogo      

www.ahkgroup.com     

    
     Rilley Chellah Mulenga
     HEAD - MATERIALS EVALUATION

     T: +260 212 226431
     M:+26076123880/ 0964084833
     E:Rilley.Mulenga@ahkgroup.com


DISCLAIMER: The information in this Internet e-mail is confidential and may be legally privileged. It is intended solely for the addressee(s).
Access to this Internet e-mail by anyone else is unauthorised.

If you are not the intended recipient, any disclosure, copying, distribution or any action taken or omitted to be taken in reliance on it, is prohibited and may be unlawful.
All results and data contained in this document are subject to our Standard Terms and Conditions and are valid only when supported by an original document.

Please visit our website at www.ahkgroup.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/4d832099-44c6-4ae1-863e-6f6781c329ean%40googlegroups.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...