Skip to main content

[MW:35854] Re: 625 Weld Overlay on SA516 Gr70 plate in 3G position

dear mohd,

1. what was base metal thickness? is PWHT done to qualified for two PWHT cycle?, 
      # hardness achieved  after pwht100-140 hv is normal.

2. if Nickle 68% is concern, try with GTAW process.

On Friday, October 17, 2025 at 8:26:35 AM UTC+3 Mohmmed Dudhiyawala wrote:
Hi Everyone,

We have encountered as PQR for Inconel-625 WOL on SA516 Grade 70 Normalized plate in 3G position.

Two Anomalies were observed: 
1. After PWHT of 120 mins, Hardness in base metal dropped from average 164 HV to average 108 HV! Has anyone observed such a drop in hardness? Is it possible? 
2. 625 WOL is done using SMAW electrode from Special Metals, the Nickel content as per consumable TC is 65%. While in WOL chemistry, 1.5mm from Top, Nickel % came around 68%. 3% Higher!! Is this possible, in any case?

Thanks in advance from your expert views.

Regards,
Mohammed Dudhiyawala, IWE

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/087ec8e7-036d-43d7-93b1-25530bd74189n%40googlegroups.com.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...