Thursday, August 25, 2022

Re: [MW:33398] Re: Weld Copper to Stainless Steel 304

You can try with inconel 625 or Nickel 200, or buttering the stainless steel with either 625 or 200 and then weld with the same consumable  to the copper
I' ve seen welding with a copper consumable in the past, but there is a high risk of hot cracks


Regards

Jurgen Prinsen IWE

Van: "Mohd Siraj" <mohd52100@gmail.com>
Aan: "materials-welding" <materials-welding@googlegroups.com>
Verzonden: Donderdag 11 augustus 2022 17:09:48
Onderwerp: [MW:33377] Re: Weld Copper to Stainless Steel 304

pl share exact specification of material to be weld with thickeness.
for any question to be answered quickly , you could provided suffiecent details so that other can understand your requirement like code interpretation querry.

On Saturday, July 30, 2022 at 5:00:55 PM UTC+3 Sohil Mehta wrote:
Dear Sir, 
Kindly suggest consumables for welding of Copper to Stainles Steel. 
Thank you.

Regards,
Sohil Mehta

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c84d8a39-6385-4d7d-9c48-df32d4658770n%40googlegroups.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...