Re: [MW:33232] Hardness Issue on weld metal

Dear Srinivas Rao,
First of all, thanks for your comments.
Consider my below reply marked in "Blue"

1. Have you checked for consumable mechanical properties with heat treatment conditions before using it PQR qualification ..? 
    Yes., MTC is attached below for your cross verification.
2. Have you verified Harness on base metal ? - No.Just followed values available in the MTC of the Pipe.
    Cross verified during the lab test, No PMI inspection done.
3. What is the tempering temperature of base material? - 630 degree C
4. Have you Checked Consumable certificates  before welding?  Are your consumables guaranteed for PWHT applications? - MTC is attached below for your cross verification.
5. Have you tried other hardness methods for cross verification?? - No.



On Thu, Jul 14, 2022 at 7:16 AM srinivas rao <engr.srini@gmail.com> wrote:
Hi Williams P Wilson,
following points to be verified before going to further details for investigation 

1. Have you checked for consumable mechanical properties with heat treatment conditions before using it PQR qualification ..? 
2. Have you verified Harness on base metal ? 
3. What is the tempering temperature of base material? 
4. Have you Checked Consumable certificates  before welding?  Are your consumables are guaranteed for PWHT applications? 
5. Have you tried other hardness methods for cross verification??

In general PHWT will not increase/affect the hardness, it is just for relieving the stresses only ,On the other hand, PWHT is usually in the same temperature range as the tempering heat treatment operates. Therefore, you should expect the same effects & results which include an increase in hardness. In such cases some of the codes and standards are recommending to control the PWHT temperatures just below 25-30 deg C below the tempering temperatures to control the mechanical properties.

you should check the filler metal certificates and data sheets for better understanding of weld metal mechanical properties before & after PWHT ,  check PMI of weld metal which will give some clarity to easily spot elements  which cause high hardness. 

Regards,
Srinivas Rao 
Welding Engineer

On Wed, Jul 13, 2022 at 3:22 PM williams p wilson <williamswilsonp@gmail.com> wrote:
Dear Experts,

During the PQR qualification of ASTM A 519, Grade 4130 , Pipe 3" x Sch XXS material hardness value in SMAW weld metal area observed in b/w 247 to 283 HV.

The required value is in blw 201 to 241 HV, Base metal hardness also is in the same range.

Preheat temperature : 200 ° C
Interpass temperature : 300 ° C (Max)

Stress relieving details as follows,
600 ° C ± 10  ° C, Holding Time : 01 Hour
Cooling Rate : 150 ° C / Hour
Heating rate : 150 ° C / Hour
Unrestricted heating up to 300 ° C
Controlled cooling upto to 300 ° C

Please reply with your valuable comments to reduce the high hardness observed in the weld metal.

Thank You & Regards
Williams P Wilson
QA/QC Engineer
Welding Inspector (CSWIP 3.1)
Cell: (+968) 94600828
P Please consider the environment before printing this message

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ7aeEfBAfaiPFbU12cS97SJOSG3-TRyHfBcbFHRzkZnGQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHdRSOPD6XkwMYcbCQjt3Saj5s_c28bygoLo%3D8r%2BZYxfwmKbVg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ6DqtLYgnutFEesZmLNqNO%3Daoie9m_XnFtgh_3ZLeKUiw%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...