Dear friend,

when ever joining of two different P nos ( 5A+4) welding, following points to be  taken care :
1, Pre heating temp shall be maintained as higher Pno ( 5A)
2, PWHT  temp shall be maintained as per higher Pno(5A)
3, Consumable shall be maintained as per lower Pno( 4)




Regards,
Sankaran.SP
Welding & Metallurgy expert.


On Wednesday, 24 February, 2021, 03:17:21 pm IST, Vishwas Keskar <vvkeskar123@gmail.com> wrote:


Apply the rules applicable for Higher P.No. of the two materials  being welded.
P no 4 to P No 5A _ Apply criteria for P NO 5A materilas.  Also consider pre heating addresed in WPS 

On Wed, 24 Feb 2021, 07:13 EmaD FaRaHanI, <emad.farahani@gmail.com> wrote:
Hello all,
As Per ASME Sec VIII, appendix R preheat criteria are determined for different PNumbers. 
But in case of welding of one BM from PNumber A to PNumber B, how can we determine the preheat criteria (temperature and thickness)?

Thanks,

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABtwbJGO7XdR27uA9Lf9%3DQF_Wj%3Dd8daCV18xeQ7_OrsCT8u%2BVQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3OQXE9F%3DvbqmGGhUMUJPaYaGsTW%3D_QnRaUSPzuuD%2BuRHA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/981665094.1697498.1614167982419%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJzm4eM8gGvoMBx4ESKLwLA5YvNb17_UDAf9uy%2BSMLd_xzcySg%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...