RE: [MW:31912] Retest of mechanical failure as per ASME Sec IX

Hi Mr Gupta,

The third para of QW 202.1 is referred and highlighted here , to discuss about this problem. According to your statement: the defect length on the failed specimen was more than 3 mm. What was the defect: lack of fusion, crack, slag inclusions, porosities.? Note all of these are welding process related and failures of test coupons due to these can't be argued and accepted.

In order to prove your point, you may have to corelate the presence of defects with NDE (RT films), provided RT was done on the coupons. According to ASME Sec-IX,RT is not mandatory for procedure coupons. ASME allows the leverage to leave the defect containing area from extracting any testing specimen.

Acceptance criteria for bend tests are quite severe,  except for failures due to sharp corners all other failures are always under the microscope and test could be rejected.

If the defects are any one those , as above , then they're process parameter related, re-welding and retesting are the only options.

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Jamie Reyes
Sent: January 3, 2021 11:47 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:31905] Retest of mechanical failure as per ASME Sec IX

 

 For such scenario that you speak of, retest is allowed And warranted per ASME IX.

 

On Sun, Jan 3, 2021 at 7:47 PM 'M R GUPTA' via Materials & Welding <materials-welding@googlegroups.com> wrote:

Dear Experts

 

Kindly suggest on below case

 

We have prepared proposed wps on the basis of that pqr was welded in one of the established classification society. Test coupon were sent in NABL lab... TPI witnessed the same...four side bend, two tensile and hardness conducted in the lab. 

 

All test pass however one of the bend tests failed due to defects length more the 3mm.

 

Then we approach TPI for re-test from the original specimen as per ASME QW202. 1 (3rd para).

 

But classification society project manager says it is a wrong practice and we will witness only new welding samples. 

 

We told him that it is written in the code and if all other test is passed then failure is not related to welding parameters.... It is particularly related to specific defect may be present at that point and that has caused failure and for that there is an option for re-test as per ASME Sec IX. 

 

Kindly suggest your opinion... And what should we do now? Because classification society is not willing to witness the re-test as per ASME sec ix. 

 

Rgds, 

M R Gupta

+91-9820604076

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/137049239.5216646.1609653065444%40mail.yahoo.com.

--

Regards,

Jamie Reyes

J.R. Machine Company, Inc.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJNUtUNnfm5%3D5c1euBjCWQgCzusNX72AFq3uJ9xy1CYtpR9iFQ%40mail.gmail.com.


Virus-free. www.avg.com

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...