Monday, January 4, 2021

Re: [MW:31908] Continuous crack in forged duplex ring by PAW process

Dear Sir,

Please find attached below the file, hope that it will help.

Best regards,

Le lun. 4 janv. 2021 à 06:58, 'Ahmed Osman' via Materials & Welding <materials-welding@googlegroups.com> a écrit :
Dears ,

ERCoCr-B need more preheat (about 400c) ... may be 1st layer not cracked as dilution with base metal change the carbides% which led to little hardness comparing with the 2nd layer... this ERCoCr-B give a very high hardness results than ERCoCr-E which have little carbon but give little hardness comparing with ERCoCr-B .

U can preheat ( but take care of duplex heating problems ) and try to keep cooling rate as low as possible .. or try one layer giving u the needed thickness ... or go to another electrode with little hardness
   

Best Regards ,
Ahmed Osman



On Saturday, January 2, 2021, 06:23:16 p.m. GMT+3, SURESH <qms.pjgpl@gmail.com> wrote:


Dear Experts
Need all your experience sharing on the below problem.

Material: ASTM A182, F55
Process: PAW
Welding: Hard facing weld overlay
Consumable ERCoCr-B (Stellite 12)
Layer deposited: 2 Layers
Deposition thick: 3 to 4mm ERCoCr-B on Base material
Interpass maintained: 150*C

During weld deposition of PAW process on 2nd layer itself crack has been propagated. We tried to rework by grinding and touch up, from that moment crack has been developed. If we tried to attend the crack place, other place are developing crack. Also now we again tried to rework, crack has been developing all the place, kindly tell me where this goes wrong?????

We are confused to do rework. As we goes deep to remove the crack, so we tried to grind 4mm deep now again deposited ER2594 by Tig process and then we follwed to weld by ERCoCr-B filler by TIG process. Again crack is developing enormously.

Please give valuable input to overcome from where we goes wrong in this?


REGARDS
SURESH 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7aa85aac-7d40-4817-8c7e-4277f7865b76n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/227958604.4151347.1609739779499%40mail.yahoo.com.


--


Mostafa DAIF  CHEF PREPARATEUR
T:  05 23 38 90 72   F:05 23 34 53 75   M:  06 61 54 12 95 ,  mostafa.daif@taqamorocco.ma
 
Jorf Lasfar Energy Company PB 99 Sidi Bouzid - El Jadida 24 000 - Maroc
http://www.taqamorocco.ma
 
TAQA MOROCCO is a member of the Abu Dhabi National Energy Company Group of companies.
 
The information contained in this communication is confidential, may be attorney-client privileged, and is intended only for the use of the addressee. It is the property of Abu Dhabi National Energy Company PJSC ("TAQA") or one of its affiliates.
Unauthorized use, disclosure or copying of this communication or any part thereof is strictly prohibited and may be unlawful.
If you have received this communication in error, please notify me immediately by return email and destroy this communication and all copies thereof, including attachments.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANRRH0J_-%2BvYQBOb2sS_Z_jrhg7V9H%3DFvseKgNQF_DefBJBphA%40mail.gmail.com.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...