Regarding to Radiographic Testing (RT) of weld
1) Does any codes / stands mentioned how to selection of film type/class like carbon steel and stainless steel?
2) On the heavy wall thickness plat 70 mm (Sphere Tank) welded by SMAW testing by PAUT were found a lot of defects but re-test by RT Ir-192 doesn't found any things, Any opinions to recommend
Thanks and Best Regards
Suchin Katavut
From: prem_nautiyal@rediffmail.com [mailto:prem_nautiyal@rediffmail.com]
Sent: Thursday, September 28, 2017 12:44 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:26838] regareding taper burning of electrode
Its manufacturing defect of consumable manufacturer.
Please tell your consumable manufacturer to replace the defective batch.
PREM S NAUTIYAL
CELL : 9769316004
From: Perumal Govindan <perumalgovindan@gmail.com>
Sent: Tue, 26 Sep 2017 11:32:54
To: materials-welding@googlegroups.com
Subject: Re: [MW:26836] regareding taper burning of electrode
Hi
I believe it's due to non concentric flux coating of electrodes. It's a manufacturing defect.
Take few electrodes from the pocket inspect visually and measure it's flux coating thickness through vernier caliper and you will find uninformed coating.
Regards
P Govindan
On Sep 26, 2017 08:10, "akshay" <akshaykulkarni.ak21@gmail.com> wrote:
when we starts welding the electrodes starts burning in taper shape please suggest improvement and reason behind it how i can overcome this problem
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Comments