Hi Duke,

 

TEG is not very corrosive, if you look at this data sheet (Watlow Corrosion Guide) the recommendation is that 316 S.S has a rating of “A-Good category ” in TEG. Please note these data are for general information and further guidance. The onus of acceptability is primarily with the process design /mechanical design  personnel of the Engineering Consultant and client’s engineers.

 

You need to validate the information with your design team.

 

At the same time it does not harm to carry out ASTM A 262 Practice –E, IGC test (the most common IGC test for austenitic stainless steels) on the plates or weld coupons. You may please discuss this issue with your AI. Most of the austenitic stainless steels if manufactured  and heat treated properly in the mill will invariably pass this test. However failure of this test may increase the potential to inspection hold ups.

 

Please check with the plate mill, on the chances of IGC practice E pass or fail criteria of the clad plates in case the AI insists the same. Same would be applicable for welding consumables also.

 

As for the statement below from UCL-32, it’s a generic statement to safeguard against improper design. It’s always a requirement in Corrosive media to match or overmatch the corrosion resistance of the base and weld metal to the process fluid involved. That’s why all the ASTM-A-262 tests (Practice A,B, C, D,E) are insisted by the designers.

 

 

Thanks.

 

Pradip Goswami, P.Eng,IWE

Welding & Metallurgical Engineering Specialist

Hamilton, Ontario, Canada

pgoswami@quickclic.net

pradip.goswami@gmail.com

ca.linkedin.com/pub/pradip-goswami/5/985/299

 

 


From: Minh-Duc Pham [mailto:mdpham1@gmail.com]
Sent: Thursday, October 22, 2015 12:41 AM
To: pgoswami
Subject: Re: FW: 23770] Weld corrosion testing on an ASME cladded pressure vessel. (UCL-32)

 

Hi Pradip,

 

No weld corrosion testing is required in the project specifications and the client confirmed it.

 

Fluid is TEG (Triethylene Glyclol).

Design pressure/temp. : 42.2 barg/100 deg.C

Internal structured packing in 316SS

 

Cheers,

 

2015-10-22 10:42 GMT+07:00 pgoswami <pgoswami@quickclic.net>:

Hi Duke,

 

Did the project specifications or design documents called for weld corrosion testing  What’s  the service media?? Appreciate if  you could  specify the design requirements.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE

Welding & Metallurgical Engineering Specialist

Hamilton, Ontario, Canada

pgoswami@quickclic.net

pradip.goswami@gmail.com

ca.linkedin.com/pub/pradip-goswami/5/985/299


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Duke
Sent: Wednesday, October 21, 2015 7:03 AM
To: Materials & Welding
Subject: [MW:23770] Weld corrosion testing on an ASME cladded pressure vessel. (UCL-32)

 

Hi all,

 

We have manufactured a glycol contactor vessel using carbon steel plate with 316SS internal cladding (3 mm).

 

DNV-GL, the vessel 3rd party inspector, is asking for a weld corrosion testing.

 

The project specification/data sheets does not request any weld corrosion testing.

 

DNV-GL interprets the UCL-32 (Weld Metal Composition) of ASME VIII div. 1 as a corrosion testing requirement.

 

UCL-32 states the following :

Welds that are exposed to the corrosive action of the contents of the vessel should have a resistance to corrosion that is not substantially less than that of the corrosion resistant integral or weld metal overlay cladding or lining. The use of filler metal that will deposit weld metal with practically the same composition as the material joined is recommended. Weld metal of different composition may be used provided it has better mechanical properties in the opinion of the manufacturer, and the user is satisfied that its resistance to corrosion is satisfactory for the intended service. The columbium content of columbium-stabilized austenitic stainless steel weld metal shall not exceed 1.00%, except when a higher columbium content is permitted in the material being welded.

 

As you see, there is no mention of any corrosion test requirement in this article and the client confirmed that he does not require any weld corrosion testing.

In the same meeting, DNV-GL confirmed that he will not accept the contactor vessel.

 

I would like to have your interpretation and experience regarding weld corrosion testing of cladded ASME vessels.

 

Thank you.

 

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/942a0fd4-5d17-4f7a-941b-6d92055003aa%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...