Dear SIvachidambaram,
You can keep it for continuously
@ 150 deg . Before that theses electrodes shall be baked @ 250-300
deg for 2 hours .Once should we take care that, the required
quantities of electrodes should be taken for baking ,then long time
holding can be avoided . And also when baked electrodes contact with
room temp for more than 4 hours ,then again re-bake required .
Shafad P.P
CSWIP3.1 /AWS -CWI
On Sun, Mar 29, 2015 at 10:51 AM, Siva Chidambaram
<mechsivachidambaram@gmail.com> wrote:
> Hi Friends,
>
> Can anybody guide me that how long shall i keep Low Hydrogen electrode on a
> Holding oven at a temperature of 150deg Cel.
>
>
> Regards,
> M. SIvachidambaram
>
> --
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-welding+unsubscribe@googlegroups.com.
> To post to this group, send email to materials-welding@googlegroups.com.
> Visit this group at http://groups.google.com/group/materials-welding.
> To view this discussion on the web visit
> https://groups.google.com/d/msgid/materials-welding/CAPJQpMVuWcr205AurnK7pcGORGKDSRon_cMDXQ9uTndK7C4ivA%40mail.gmail.com.
> For more options, visit https://groups.google.com/d/optout.
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOWuSzFGN90fUHLLyoPtH8-y7%2B%3D%3DnVdOya0RkDp17s3OuqEEwQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Subscribe to:
Post Comments (Atom)
Re: [MW:35686] HDPE WPS
Refer ASME SEC IX There is separate chapter for Plastic welding . Based on that you have to prepare Sent from my iPhone On 21 Jun 2025, at...
-
Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? ...
-
Definition of buttering from ASME Section IX, QW/QB-492 Definitions: Buttering: the addition of material, by welding, on one or bot...
-
Section I. PRINT READING 3-1. GENERAL a. Drawings . Drawing or sketching is a universal language used to convey all necessary information to...
No comments:
Post a Comment