Preheating is a must for these materials, because of carbon content (nearl %0,40) 300 C preheating is necessary and low cooling rate. After welding it's better to use pwht (normalizing)
ER80S-B2 - (CrMo1), E8018-B2 (CrMo1) can be used or some of dissimilar consumables, such as ER307 (18 8 Mn), ER312 (29 9)

Best regards.
Murat

27 Mart 2015 Cuma 04:37:55 UTC+2 tarihinde Pravin yazdı:
Dear experts,

Kindly advice which welding consumable should I select for following material:

1. 4140 SMAW,GTAW,FCAW,SAW

2. 4130 SMAW GTAW FCAW SAW

Since above listed both material are high tensile material, is there any special heat treatment or welding condition need to be taken into consideration for better mechanical result.

Kindly advice

Pravin
Singapore

Sent from my iPhone

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/f93e76b3-9c4b-4a33-a520-bf34575cd505%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...