Dear experts,
Sorry for the late reply.
We cant afford for NDT.
Also UT is not possible due to the profile of the job.
But we have an internal testing lab where i could do a destructive testing free of cost.
Please find the attachments with respect to the macro test which we have conducted.
After etching the weld test piece we have drawn a triangle from the weld centre line with included triangle 60 degree.
Our lab report tells if L>12mm & A>1mm then it is a proper fused weld.
If L<11mm & A<1mm then there is a side wall lack of fusion.
Please give your comments Is IT correct or not?
with regards,
Saravanan
On Mon, Jan 20, 2014 at 2:45 AM, Mohammad abu eassa <mr.mohammad.eassa@gmail.com> wrote:
you can get it easy using UT--
On Thursday, 9 January 2014 10:50:28 UTC-8, sara vana wrote:Dear experts,
How to measure side wall lack of fusion by destructive testing.
Component : butt welding of plates
Joint configuration : groove weld with included angle sixty degreeTo post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


Comments