What is the design temperature ?   what was the impact test temperature for PQR qualification vs. the AWS classification used E 7018/E-7018-1?
 
Usually these electrodes are manufactured to meet dual certification i.e,7018/7018-1 and are tested for impact @ -45Deg C. If such electrode is used for production weld then no issues.
 
Otherwise E-7018(certified for impact @-29 Deg C) is not matching to SA 333 Gr6 (guaranteed impact -46 Deg C) base metal.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Richard robes
Sent: Sunday, February 16, 2014 9:59 PM
To: materials-welding@googlegroups.com
Subject: [MW:20114] Use of E7018 instead of E7018-1 - Low Temperature Pipe.

Gents,
What all are the practical issues if someone has welded low temperature A333 Gr.6 pipe with wrong electrode E7018 instead of E7018-1.

Regards
Richard

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35725] Dismillar material Welding

Dear experts,  In my Hydro Electric Project  materials using A517Gr.F and A537CL-II.  For A517Gr.F using E 11018M and A537CL-II using E 9018...