Inspection Connection: Radiographic and ultrasonic weld inspection

 

Inspection Connection: Radiographic and ultrasonic weld inspection

Establishing weld integrity without destroying the component

By Tony Anderson, Contributing Writer
February 14, 2002

This article outlines the differences in radiographic and ultrasonic weld inspection, the two most common methods if nondestructive testing. It gives an overview of both methods, including how they are used.

Radiographic and ultrasonic weld inspection are the two most common nondestructive testing (NDT) methods used to detect discontinuities within the internal structure of welds. The obvious advantage of both of these testing methods is their ability to help establish the weld's internal integrity without destroying the welded component.

Radiographic Testing

Radiographic testing (RT) usually is suitable for testing welded joints that can be accessed from both sides, with the exception of double-wall signal image techniques used on some pipe. Although this is a slow and expensive NDT method, it is a dependable way to detect porosity, inclusions, cracks, and voids in weld interiors.

RT makes use of X-rays or gamma rays. X-rays are produced by an X-ray tube, and gamma rays are produced by a radioactive isotope. The basic principle of radiographic weld inspection is the same as that of medical radiography. Penetrating radiation is passed through a solid object (in this case, a weld rather than part of the human body) onto photographic film, creating an image of the object’s internal structure on the film.

The amount of energy absorbed by the object depends on its thickness and density. Energy not absorbed by the object causes exposure of the radiographic film. These areas will be dark when the film is developed. Areas of the film exposed to less energy remain lighter. Therefore, areas of the object where the thickness has been changed by discontinuities, such as porosity or cracks, will appear as dark outlines on the film. Inclusions of low density, such as slag, will appear as dark areas on the film, while inclusions of high density, such as tungsten, will appear as light areas.

All discontinuities are detected by viewing the weld shape and variations in the density of the processed film. This permanent film record of weld quality is relatively easy to interpret if personnel are properly trained. Only qualified personnel should conduct radiography and radiographic interpretation because false readings can be expensive and can interfere seriously with productivity, and because invisible X-ray and gamma radiation can be hazardous.

Ultrasonic Testing

Ultrasonic testing (UT) can be used on ferrous and nonferrous materials and often is suited for testing thicker sections accessible from one side only. In general, it can detect finer linear or planar defects than can RT.

UT makes use of mechanical vibrations similar to sound waves but of higher frequency. A beam of ultrasonic energy is directed into the object to be tested. This beam travels through the object with insignificant energy loss, except when it is intercepted and reflected by a discontinuity.

The ultrasonic contact pulse reflection technique is used in UT. This system uses a transducer, which converts electrical energy into mechanical energy. The transducer is excited by a high-frequency voltage that causes a crystal to vibrate mechanically. The crystal probe becomes the source of ultrasonic mechanical vibration. These vibrations are transmitted into the test piece through a coupling fluid, usually a film of oil, called a couplant.

When the ultrasonic waves pulse strikes a discontinuity in the test piece, it is reflected back to its point of origin. Thus, the energy returns to the transducer. The transducer now serves as a receiver for the reflected energy.

The initial signal, or main bang; the returned echoes from the discontinuities; and the echo of the rear surface of the test piece all are displayed by a trace on the screen of a cathode-ray oscilloscope. The detection, location, and evaluation of discontinuities become possible because the velocity of sound through a material is nearly constant, making distance measurement possible, and the relative amplitude of a reflected pulse is more or less proportional to the size of the reflector.

One of the most useful characteristics of UT is its ability to determine the exact position of a discontinuity in a weld. This testing method requires a high level of operator training and competence and depends on establishing and applying suitable testing procedures.

Tony Anderson is a regular contributor to this section and technical services manager with AlcoTec Wire Corporation, 2750 Aero Park Drive, Traverse City, MI

 

Tony Anderson
Technical Services Manager,
AlcoTec Wire Corp.

Tony Anderson is a regular contributor to this section and technical services manager with AlcoTec Wire Corporation, 2750 Aero Park Drive, Traverse City, MI 49686-9263, phone 800-228-0750, fax 231-941-9154 Web site
www.alcotec.com.

Tony has a background as a certified welding inspector, welding engineer-quality manager, and NDT manager. He also serves as chairman of The Aluminum Association Technical Advisory Panel for Welding and Joining, vice chairman of the AWS D1G Subcommittee 7 on Welded Aluminum Structures, and a member of Practical Welding Today's Editorial Review Committee.

tanderson@alcotec.com

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...