[MW:537] Re: 533] Filler metal for P 11 (O/L SS 347) to P8

This is a typically rare case. You may follow as follows:

1) Buttering on P-11 material by inconnel (ENiCrFe-3 is the most
economical). Minimum thickness should be 4.8 mm.
2) PWHT of the buttering. (Local PWHT is desirable if whole bonnet is not
subject PWHT)
3) Welding of LWN nozzle (I suppose it will be set-on type) onto the
buttering. (Be careful not to touch the base metal P-11 during the final
welding)

If it is not practicable or if process/project specifications allow
indexcriminate PWHT of the SS 321 material, you may avoid buttering (step-2
above)

By the way, what is the design temperature for the Tube-side? (There is
also a restriction in code for inconnel filler.)

Best regards,

Prasad Joshi
e-mail: pjoshi@technip.com
Phone: +971-(0)2-611-6643



gopal sankar
<gopalsankar@yaho
o.com> To
Sent by: materials-welding@googlegroups.com
materials-welding cc
@googlegroups.com
Subject
[MW:536] Re: 533] Filler metal for
30/01/08 07:10 AM P 11 (O/L SS 347) to P8


Please respond to
materials-welding
@googlegroups.com


In the above query the thickness of weld neck & nozzle has not been
mentioned and assume that the connection is between the nozzle pipe & weld
neck flange.If there is no PWHT as per design requirements then root as
well as final pass welding can be carried out using ER347 +E347 due to
homogeneuous layer present. Welding final layer with Inconel will not give
have any positive impact rather the chance pf cracking is not ruled out due
to differential thermal expansion of P11+SS347+Inconel.Either full welding
with 347 or Inconel will be a better option.

with regards,
gopalsanakr
DM(ES-Inspn)
CPCL
Chennai

"Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com> wrote:
Is this vessel subjected to PWHT?
I assume it should be, also assuming it is a stub in type connection, then
use ER347 + E347 for joining weld overlay portion to LWN (i.e inside weld
of nozzle), and may use Inconel consumables ERNiCr3+ENiCrFe-2/3 for weld
on ouside (i.e fillet joining P11 to F321 neck)

From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of Desai Jignesh
Sent: Tuesday, January 29, 2008 2:46 PM
To: materials-welding@googlegroups.com
Subject: [MW:533] Filler metal for P 11 (O/L SS 347) to P8

Dear Member,

Can some body give his/her opinion for filler metal of following
condition?

Branch connection (Tube Side) between LWN flange (Material SA 182 F321) to
SR Nozzle (SA 182 F11 CL 2 + Weld Deposit 347 SS).

Service is Hydrogen.

Operating Wall Temperature - Tube Side is IN 372 C & Out 225 C.

Also recommend the filler metal for the first layer of weld deposite.

Thanks in advance

Jignesh

Looking for last minute shopping deals? Find them fast with Yahoo! Search.

Save a tree...please don't print this e-mail unless you really need to.

Save a tree...please don't print this e-mail unless you really need to.


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...