Re: [MW:33185] RE: PWHT Segment Wise for 9 Meter Dia Vessel

Straight to the point Mr. Vishwas.

Thanks & Regards

J.Gerald Jayakumar



On Sunday, 26 June, 2022 at 10:54:11 am GMT+4, Vishwas Keskar <vvkeskar123@gmail.com> wrote:


Dear Vishal 
As I understand  correctly , the vessel circumference is 9 mtr  and  your query is that you want to carry out the PWHT of the Circumferemtial seam in segments.

The answer is No . You have to carry out PWHT  of  ENTIRE Circumferencial joint in ONE cycle.
You can do it by LOCAL PWHT method by wrapping Electric Resitance Coil on job and attaching job thermocouples.

Many HT contracter are doing such type jobs regularly.
Thanks 
Vishwas Keskar 
IWE- International Welding Enginner

On Sat, 25 Jun 2022, 20:21 , <pgoswami@rogers.com> wrote:

Hi,

It's allowed by Sec VIII, DIV1. Please see the highlighted clauses as below.

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

UW-40 PROCEDURES FOR POSTWELD HEAT TREATMENT:

From: vishal hirde <vishalhirde1988@gmail.com>
Sent: June 25, 2022 8:24 AM
To: materials-welding@googlegroups.com
Subject: PWHT Segment Wise for 9 Meter Dia Vessel

 

Dear All,

 

We are fabricating a Vessel of Diameter 9 Meter at Site, requires PWHT: Material Grade SA 516 Gr. 70.

 

 For Circumferential Joint PWHT can it be performed Segment Wise as diameter is more??

 

Pl. Confirm as per ASME Sec VIII Div 1 can it be done in Segment Wise. 

 

--

With Best Regards,

Vishal Hirde




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAAD9ib%2BzVU4dRb/ePF01LBnGAQAAAAA%3D%40rogers.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3Pk96%3DsLj8Qgn%2B17h7%2B5A3t7bYEJKFGBnBcm4b4kO7tRA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...