Re: [MW:33153] RE: 33147] SA 387 GR 11 CL2 and SA 387 GR 22 CL2

Hi!
my experience 
Normalising of weld of higher thickness reduces the YS and UTS cosiderably 
as D/End manufacturer invariably ask for repeated Normalising during forming  ( say 2 to 3 times) and they take soaking temperature to higher side i.e above  930 c
Therefor it is recomended to go for Total Hot forming of D/E ( with no weld seam)
and then after go for Nr +T  to get back required properties
or Go for Crown and Petal type D/E having   which does not req NR +T of Weld

(As its total LM parameter No increases)

Regards


 

On Thursday, 16 June, 2022, 08:27:27 pm IST, <pgoswami@rogers.com> wrote:


You should use E 8018 B2 or 8018B3L as SMAW consumables. SAW wire flux combination matching SMAW chemistry is also to be considered. If the hardness requirement is in place, then 8018 B3L would be advisable.

On Cr-Mo steels normalizing may sacrifice the Charpy impact , hence consumable with extra Mo(B3Lgrades) may be of help.  

 

Pradip Goswami.P.Eng, IWE.

Independent Welding & Metallurgical Engineering Specialist

Saudi Aramco Approved Designated Project Welding Engineer (DPWR)

Qatar Petroleum Approved, SME-Materials & Corrosion Engineering.

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@rogers.com,pradip.goswami@gmail.com

Cell/Whasapp:1-905-9793232

 

From: materials-welding@googlegroups.com <materials-welding@googlegroups.com> On Behalf Of Vishwas Keskar Welding Manager WELDING
Sent: June 16, 2022 2:23 AM
To: Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:33147] SA 387 GR 11 CL2 and SA 387 GR 22 CL2

 

Experts 

 

The dished end is to be fabricated with one number Chordal seam  for MOC of 

1) SA 387 GR 11 CL2

2)SA 387 GR 22  CL2

 

One  chordal seam in dished end is coming due  to plate  size( width) limitation  and the  diameter required of  dished end. So butt joint welding is to be done  followed by NDT .

 

Hot forming is planned . After forming is completed, separate   Normalizing and tempering Heat treatment is required as per Client specification.

 

PQR is to be established as per ASME SEC IX  .

Pl. suggest suitable consumable  and maintain strength 

 

Pl. share experience if any 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bd3a1f1c-6422-4640-985a-d05964ed96d5n%40googlegroups.com.




AVG logo

This email has been checked for viruses by AVG antivirus software.
www.avg.com


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAuAAAAAAAAABVPzeizzeRJsiPziIE5jXQBAMO2jhD3dRHOtM0AqgC7tuYAAAAAAA4AABAAAAB8WX7Ei11gSJhbEsWBENQ9AQAAAAA%3D%40rogers.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...