Skip to main content

Re: [MW:32658] Acceptance criteria for PMI of dissimilar metal weld

Dear Mr. Govindan, 

Do you mean in this case, acceptance criteria shall be in red color as below ? 

6Mo weld to 6Mo
Cr Ni Mo
A312 S31254 (6Mo) 19.5-20.5 17.5-18.5 6-6.5
A312 S31254 (6Mo) 19.5-20.5 17.5-18.5 6-6.5
ERNiCrMo-3 20-23 58 min 8-10
Weld metal required 19.5 17.5 6



Vào Th 5, 9 thg 12, 2021 vào lúc 13:25 Perumal Govindan <perumalgovindan@gmail.com> đã viết:
While welding dissimilar materials, usually lower grade properties shall be acceptable and its a normal industrial practice.

For more information, pease refer your welding specifications of.your project.

Regards 
P Govindan 

On Thu, Dec 9, 2021, 11:39 AM anhtrangnghieng <anhtrangnghieng@gmail.com> wrote:
Dear Experts, 

We have a welded joint: stainless steel type 6Mo UNS S31254 using filler metal ERNiCrMo-3. What would be the chemical requirements criteria ( Cr, Ni, Mo)  be for PMI on this joint? Any standard/ code for reference? 

--




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADOyxJi%2BOSmeuJhmc8e-hvB8c8hMHnzXBMAkX8WuJ9tzJhdrnw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANiuf9d6KtR%3Dy-%2BggtZoFBRrAHxA%2BvmuOz4x5pnsHn%2BMDAQhKQ%40mail.gmail.com.


--




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADOyxJhrsUFqzK48SoWsjLmhvxt3ytGgE8m9JxNks%2BeFhC6nug%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...