Skip to main content

Re: [MW:31201] Re: Annealing and Normalizing temperature for F316 & SS410

Dear Experts
Thanks for the valuable feedback. Will check as per the suggestion


Regards
Suresh

On Sun, 26 Jul 2020 at 19:49, Vanchinath S.A. <vanchinaths@gmail.com> wrote:
carryout annealing at 850 degC with furnace cooling 30 degC/hr max to achieve hardness in range around 160 BHN. As per spec max hardness permitted in annealed condition is 223 BHN.
quenching at 980 degC followed by tempering at diff temp is for obtaining higher hardness.
vanchinath

On Sat, Jul 25, 2020 at 8:05 PM SURESH <qms.pjgpl@gmail.com> wrote:
Hi My question is what is the suggested annealing temperature for .ASTM A473 Typ410 grade. If your refer the standard of  ASTM A473, Table 2 they have given condition like A,1,2,3.

So if it is annealed condition what is the suggested temperature to achieve 223BHN?


Note: Refer attachment

Regards
Suresh
On Saturday, 25 July 2020 at 09:24:17 UTC+5:30 ramink...@gmail.com wrote:
If this is the TDC for raw material as per contract, then you have to find a supplier who can provide it unless you can prove that it would cause problems during fabrication or operation. And that is why I told you to provide us with more details. 
Then you need a qualified engineer who reviews all the documents and is able to get into a discussion with your client to find out whether other alternatives are acceptable or not. I do not think you can do it via online inquiries; you need to hire someone to do this for you... 

Ramin  Kondori
Sr. QA/QC & Welding Engineer
-----------------------------------------------------------
PG-Dip. in Welding Engineering (IWE  AT  0070)
BSc. in Civil Engineering (IUT)
BGAS Painting Inspector
ASNT Level I&II
                        
IIW-Logo-Colour-small


On Fri, Jul 24, 2020 at 7:45 AM <sathis...@gmail.com> wrote:
Dear Mr.Ramin Kadori.

My customer is given TDC for annealing at 955 C but raw material supplier is suggesting that they do only with 850 C. Its not for fabrication, to give raw material into finished component by machining. Required hardness is 160 BHN

As per ASTM A473, Grade/Typ. 410 can be supplied as per the following conditions:




Condition A refers to annealing. (ASTM A473 mentioned with A, 1,2,3,). In this case how to determine the Annealing temperature?


My requirement is to get hardness of 160BHN

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/bbae9d88-9b64-421b-9dc6-8b8c357732d9n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CA%2B6Tn1JoRSNXbD3qtu0SWG3js%3DMV23Xq9wLuWD4UjGv9LOJ%2Bvg%40mail.gmail.com.


--

Thanks and Regards,

S.SATHISH KUMAR

Packings & Jointings Gaskets Private Limited 

No:347, North Phase,3rd Street ,SIDCO Industrial Estate,

Chennai 600098,

India

Tel: +91-44-48627746

Mob : 9841788979

Email : qms.pjgpl@gmail.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJFfihwu0NDLRfK%2BmLXoJfKiqm%2BpGyEXDNFDgB9uCd%2BoqoehVw%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...