According to UG-79 Heat Treatment is required for Cold Forming heads when:
A- Extreme Fiber Elongation is more than 40%
B- Fiber elongation is more than 5% and any of the following condition exist:
- Impact Test is not exempted according to UCS-66
- Heads for lethal service vessel as restricted in UW-2
- Head plate thickness before forming is 16 mm
- Thickness reduction at any location after forming is more than 10% of actual thickness where extreme fiber elongation is more than 5%
- Forming Temperature between 120-480 deg. C
You may calculate fiber elongation from formula given in Table UG-79.1 or better to consult with pressure vessel designer for this calculation.
(Heat Treatment when applicable will perform by following UCS-56 requirements)
Hot Formed heads in no case does not require heat treatment after forming.
Regards,
On Sun, Mar 31, 2019 at 7:26 PM George Dilintas <dilintas@gmail.com> wrote:
Wrong,you should read UCS-79 carefully. The HT is a function of P-No and extreme fiber elongation, and service conditions.UCS is applicable for carbon steel materialsFor high alloy (example stainless steel) pls refer to UHA-44For enhanced ferritic steels pls read UHT-79.Friendly advise: read the Code carefullyĪ£ĻĪ¹Ļ ĪĻ Ļ, 31 ĪĪ±Ļ 2019 ĻĻĪ¹Ļ 5:34 Ļ.μ., Īæ/Ī· Brijesh Maurya <brijeshmaurya492@gmail.com> ĪγĻαĻε:thickness above 16 mm as per UCS-79 of ASME sev.VIII div.1--On Thu, Mar 28, 2019 at 4:53 PM vikram saipogu <saipoguvikram@gmail.com> wrote:Dear All,--Under which Condition,Heat Treatment is mandatory for dish end ?Thanking you.Best Regards,Vikram Saipogu
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
----Dr. Georgios Dilintas,Dipl. Ing. In Aeronautic and Space EngineeringPh.D in Mechanics of Solids - Computational MechanicsA.I.S, A.N.I, IRCA Lead AuditorWelding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Comments