Re: [MW:29502] Aluminium Bronze welding

You can maintain flow rate of argon gas @ 15 LPM.

Regards

Prem Nautiyal


PREM S NAUTIYAL
CELL : 9769316004





From: Mohammed afzal Khateawdi <afzal8880@gmail.com>
Sent: Sun, 21 Apr 2019 18:58:51 GMT+0530
To: materials-welding@googlegroups.com
Subject: Re: [MW:29500] Aluminium Bronze welding

Hi....Prem 

Hereafter considering below points as per you, Plz share with us what was flow rate l/min for Argon gas ?

Use 99.995% pure argon

Preheat 150 – 180 ˚C

Inter pass temperature @200 ˚C

Inter run cleaning is very important to remove surface oxides 

Thanks & Regards,




On Tue, Oct 2, 2012 at 6:51 PM prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
Hi
 
Why dont you read the subject line and the past discussions before posting your query ?
We are discussing Aluminium bronze. Dont create confusion ..
 
Regards
 
Prem Nautiyal


--- On Tue, 10/2/12, Ashish Pathrabe <darkash6633@gmail.com> wrote:

From: Ashish Pathrabe <darkash6633@gmail.com>
Subject: Re: [MW:15444] Aluminium Bronze welding
To: materials-welding@googlegroups.com
Cc: "kannayeram gnanapandithan" <kgpandithan@gmail.com>
Date: Tuesday, October 2, 2012, 1:25 PM

Dear Esperts:=
 
You are replying for Aluminium Bronzee or for monel Welding.
 
pls , clear the confusioo
 
Ashishj

On Sun, Sep 30, 2012 at 9:14 PM, prem nautiyal <prem_nautiyal26@yahoo.com> wrote:
No doubt Helium+Argon mixture will give better fusion and penetration, but i have welded lot of Al-Br with Pure argon.
Hel+Ar mixture is a costly affair.
Also preheat is must.
 
Regards
 
Prem Nautiyal


--- On Sun, 9/30/12, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:

From: kannayeram gnanapandithan <kgpandithan@gmail.com>

Subject: Re: [MW:15374] Aluminium Bronze welding
To: materials-welding@googlegroups.com
Cc: prem_nautiyal26@yahoo.com
Date: Sunday, September 30, 2012, 1:13 PM


use helium+argon mixture
need not preheat
clean properly
pandithan
In-charge/wt
Cethar

On 9/24/12, bo gyi <aungbomyint@gmail.com> wrote:
> Hi
>
> Base material is B171 C61400 & 99.9995% argon is used.
>
> Regards,
>
> On Friday, September 21, 2012 10:01:11 PM UTC+8, prem nautiyal wrote:
>>
>>
>> Hi
>>
>> Its not an easy task to weld Al bronze.
>> What is your base material grade ?
>> Clean base metal and filler wire before welding.
>> Use 99.995% pure argon.
>> •Preheat 150 – 180 ˚C
>> •Inter pass temperature @200 ˚C.
>> •Inter run cleaning is very important to remove surface oxides
>>
>> Regards
>>
>> Prem Nautiyal
>> Cell: 9769316004
>>
>> --- On *Fri, 9/21/12, bo gyi <aungb...@gmail.com <javascript:>>* wrote:
>>
>>
>> From: bo gyi <aungb...@gmail.com <javascript:>>
>> Subject: [MW:15353] Aluminium Bronze welding
>> To: material...@googlegroups.com <javascript:>
>> Date: Friday, September 21, 2012, 7:46 AM
>>
>> Hi Sirs,
>>
>> Currently, I am doing procedure for Aluminium Bronze (61400) using GTAW (
>>
>> ERCuAl-A2) process by Argon shielding gas but found that fusion of filler
>>
>> metal & base metal is not nice.
>>
>> Can anyone advice?
>>
>> Thanks and regards,
>>
>> Bo
>> --
>> To post to this group, send email to
>> material...@googlegroups.com<javascript:>
>> To unsubscribe from this group, send email to
>> materials-weld...@googlegroups.com <javascript:>
>> For more options, visit this group's bolg at
>> http://materials-welding.blogspot.com/
>>
>> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>>
>> The views expressed/exchnaged in this group are members personel views and
>>
>> meant for educational purposes only, Users must take their own decisions
>> w.r.t. applicable code/standard/contract documents.
>>
>>
>>
>>
>
> --
> To post to this group, send email to materials-welding@googlegroups.com
> To unsubscribe from this group, send email to
> materials-welding+unsubscribe@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>
>
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https:roups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...