Once our shop got a relax from client to keep it as long as one week if the storage was done with assurance that relative humidity would be low and not create risk of cracking due to water.

What we did during that time was using heater in storage shade and monitoring humidity.

Anyhow,  no body is comfortable to see 15E welded joint stayed without PWHT too long.  PT/MT and volumetric inspection after PWHT is highly recommended.

Regards,

C.Nopadon

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of pgoswami
Sent: Friday, February 26, 2016 11:59 AM
To: materials-welding@googlegroups.com
Subject: [MW:24374] RE: 24373] Time between Hydrogen Bake Out and PWHT

 

Hi Mac,

 

One week without PWHT on 3.5" think Grade -91 Steel is too long. In spite of hydrogen bake out one may get cracking. Did any one check the hardness of weld and HAZ by any means (just for curiosity??).

 

Also prior to the DHT the welds should be cooled to Mf   temperature which is generally  the ambient temperature. In absence of it full martens tic transformation won't happen causing poor creep strength in these steels. DHT may be adopted before the PWHT, however not advised to delay PWHT so long.

 

It's worth looking at.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgoswami@quickclic.net

pradip.goswami@gmail.com

 

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com]
Sent: Thursday, February 25, 2016 3:47 PM
To: Materials & Welding
Subject: [MW:24373] Time between Hydrogen Bake Out and PWHT

 

Dear Sirs,

We welded a 15E Pipe material (16 inch - 87mm thickness).
Our procedure will be preheated with 205 deg centigrade then welding and will be
( hydrogen ) bakeout and perform PAUT, If accepted in PAUT, immediately followed
by PWHT and will perform MT.
Process is B31.1

The joint has been accepted by PAUT, my query is, how long should be acceptable if there is a delay in performing PWHT?
Right now it is almost 1 week that the welded joint is not yet PWHT.

Need your advice.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/2273403b-7345-464c-8e91-93d53134f4f8%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAAClD1TdHQKRLquEJzyVMUawBAAAAAA%3D%3D%40quickclic.net.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...