Hi Mr.. Rao,
 
These black spots are essentially the products of contamination in the weld metal.There may not be a single reason towards this .It may happen as follows:-
  • Welding Fillers :- The drawing lubricants e.g graphite could contaminate the welds and cause  these spots to be formed. Through acetone cleaning of all the fillers should be done before welding. Also fillers with oxidized tips should be used following  removal of the oxidized tip(by cutting).
 
  • Shielding gas: check the purity of the gas, it should be 99.95% or more.  Premixed gases say Ar+N2 may contain traces of moisture , which  may increase the oxygen potential and the resultant oxidation of the puddle. As you said  earlier the "O2" content was  well below 0.2%.. Assuming the fact that  for shielding gas everything was under control it would be always advisable to check the right purity of the shielding and purging gas, prior to welding.
 
  • The condition of the pipes:- Duplex pipes should always be pickled  and cleaned at the mill. If not done at the mill, it's preferred to pickle the pipes and remove the excess scale or oxides in the fabrication shop. Usually such oxides could be very microscopic and very difficult to remove by grinding. Excess oxides may introduce contamination in the weld.Also cross contamination during grinding could harm the welds.
 
The dark spots are bad , with potential for pitting during procedure qualification testing or while put in service.
 
Let me know if it helps.
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: Vasantharao [mailto:vasantharao@yahoo.in]
Sent: Wednesday, February 12, 2014 11:57 PM
To: pgoswami
Subject: Fw: Black spots on DSS Weld Joints.


Dear sir,

Can you give you suggestions on DSS dark spots as group member are not responding.

Is there any problem with dark spots. Why it forms. 

regards
P.Rao

On Wednesday, 12 February 2014 1:38 PM, Vasantharao <vasantharao@yahoo.in> wrote:
Dear Experts,

We observe Dark spots on Welding of Duplex Stainless Welds.  

Material is : UNS S31803 ,  Filler Wire for root - ER2594, rest ER2209.

Sample pictures are attached for reference.

Oxygen level in shielding / Purging maintained well below 0.2%.

Interpass <150 Deg.C

Pl. share your valuable information.

Thank you.

P.Rao


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...