it can go below 620 °C, if you meet all the requirements of para A 2. 1. 4. however ensure that your simulation and actual PWHT temp should in the same range. if plate mill can't guarantee the plate at 620 °C, you can't go for product PWHT beyond 600 °C

dished ends are manufactured by the mill? if not what is the final treatment by dished end manufacturer. is it NACT or normalizing?

NACT can be accepted for NACE service, as manufacturer will certify it as NT. 


On 23 January 2014 12:51, Jignesh Desai <jignesh.desai.met@gmail.com> wrote:
One query related to acceptance of NACT plates instead of only Normalised.

For Shell:
SA 516 GRADE 70 - SOUR - NACE  - SEC VIII-II
THICKNESS - ABOVE 100 MM
PWHT TEMP = 621° C - MIN AS PER NACE
SIMULATION - NORMALISING + 3 PWHT CYCLE


For Heads:
SA 516 GRADE 70 - SOUR - NACE -SEC VIII-II
THICKNESS - ABOVE 100 MM
PWHT TEMP = 621° C - MIN AS PER NACE
SIMULATION - NORMALISING+NORMALISING + 3 PWHT

Que:
 
1. IF HEAT TREATMENT IS CARRIED OUT IS NACT INSTEAD OF NORMALISING THEN MILL IS GIVING THE GUARANTEE FOR ABOVE SIMULATION.

2. ............CAN WE REDUCE THE PWHT TEMPERATURE (LESS THAN 621° C) UP TO WHAT LEVEL ???, ............As some of the Mills are giving guarantee of 4 PWHT cycle with 600°C

Regds/Jignesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...