[MW:19885] RE: 19876] Re: Welding UNS S31254 to UNS S31254

Hi Prabhu,

625 Filler contains fairly high percentage of "Nb"(please see below)

The presence of Nb causes problems that may place restrictions on the weld procedures. Nitrogen can diffuse rapidly from the 6%Mo HAZ to the weld metal and result in the formation of niobium nitrides at the weld deposit & fusion boundary, leading to some loss of ductility and corrosion resistance.

If the failures are in side bends test, then Nb  in weld metal  should be restricted to minimum or Nil content.

It would be good to know what's the real problem.

Thanks

 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of prabhu
Sent: Thursday, January 16, 2014 10:56 PM
To: materials-welding@googlegroups.com
Subject: [MW:19876] Re: Welding UNS S31254 to UNS S31254

Dear All,

ER NiCrMo-3 result are dood for lower thickness but for higher thickness i am getting problem. I am welding 10-16 mm thick plates please guide welding parameters for the same.

On Friday, November 15, 2013 3:28:52 PM UTC+5:30, prabhu wrote:
Dear All,

Can you guide me for selecting TIG filler wire for SMO 254  UNS S31254  to  UNS S31254 plate thickness 10mm
and in preparing WPS for same with parameters inputs.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...