 In the first part - ER 70S-6 & ER 70S-2:     

S-6: contains very high Manganese & Silica content which will act as de-oxidizers and could    
       be used along with CO2 as shielding gas. Radiographic quality of weld is not mandatory.
       Recommended for GMAW (MIG & MAG) process.
 
S-2: contains limited amount of Mn & Si, but has additional elements like Zn – Al – Ti, which will
       act as deoxidizers and could be used along with Argon ( or) with Ar (+) O2 as shielding gas.
      100 % radiographic quality of weld is obtainable. Recommended for GTAW (TIG) process.
 
In the second part i.e., with ER 70S-6:
The said golden spots are nothing but non-metallic slag spots, caused by the reaction of excessive Manganese (Mn)
used as a de-oxidizer in S-6 wire and reaction of Mn (+) Oxygen, which is transferred through CO2 shielding gas.
 
It will not stick to weld surface and could be removed easily by hand / power brushing and it is a general post weld
practice if surface painting  to be done. But, spots can be controlled through proper selection of Voltage / current
ratios, by using Ar (+) CO2 mixture gas and good bead ripple finish.
 
If required you can use ER 70S-2, but it is 3 times expensive to S-6 wire. Alternatively, S-3 also could be used with
Argon gas.
 
Sridhar.
 -------------------------------------------------------------------------------------------------------------------------------------------------------------------------------
ram Yadav <yadav.vikram394@gmail.com>
To: materials-welding@googlegroups.com
Sent: Saturday, 28 December 2013 9:12 AM
Subject: [MW:19730] Re: DIFFERENCE BETWEEN ER70S-2 &ER70S-6

Dear Sir,
 
I am using ER70S-6 for GMAW. But found golden spots after welding. Are these golden spots Silicon Oxide or somthing else.
These golden spots causes problem during paint as its a not metal it is not covered in CED bath. I always found these spots more brighter after the paint baking.I want to eleminate this probem.
 
So can i switch to any other wire with less silicon composition or there is any better alternate available.
 
Please Suggest.
 
 
 
 
On Monday, November 26, 2012 1:49:14 PM UTC+5:30, vinu raveendran wrote:
Dear Members,

I would like to know difference between ER70S2 &ER70S6?
What does "2" and "6" mean in them and which welding process we use them?

Thankyou! 

--
VINU RAVEENDRAN
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


No comments:

[MW:35668] Selection of Filler/Electrode.

Dear Gentlemen, Kindly advise me as we have tube to tubesheet joint. Tube moc is incoloy 800 And tubesheet moc is F53 SDSS (Super duplex sta...