[MW:19704] RE: CRACKS IN SKIRT WELD

Hi Lassad,
 
Head to skirt weld joint is one of the complex weld joints in any pressure vessel. In addition to hoop stress from the resultant pressure there's constant dead weight load of the vessel/equipment on the head to skirt weld. If the vessels are subjected to cyclic loading shirt welds could fail prematurely.
 
Attached are 2 schematics on head to skirt welds. The first one a fillet weld is commonly used, while the second design is recommend for better design and integrity. Which design was used for the LPG spheres ?
 
If the cracks are removable by grinding and blending then that should be the first option. Following removal perform WFMPI of the weld seam  to ensure no cracks are left behind in addition to the ones removed.
 
If it calls for deeper grinding and weld repair, there the rules of the respective design codes should be followed. Head to skirt weld would require same or more care than the  girth welds, in terms of preheating , interpass temperature control etc.
 
If PWHT following weld repair is  required by the design code that such PWHT should be  on the total circumferential welds or as accepted by the AI.
Local or spot PWHT could create distortion. However for C-Mn steel as PWHT(SR) is usually done well below the AC1 temperature(723 Deg C)there are a number of ways to control the distortion.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
              


From: Lassaad Mokrani [mailto:lassaad.mokrani@gmail.com]
Sent: Monday, December 23, 2013 3:03 AM
To:  pgoswami@quickclic.net 
Subject: Fwd: CRACKS IN SKIRT WELD

Dear Mr.Pradip,
Could you please give me your valuable inputs on that matter?
Many thanks

---------- Forwarded message ----------
From: Lassaad <lassaad.mokrani@gmail.com>
Date: 2013/12/22
Subject: CRACKS IN SKIRT WELD
To: materials-welding@googlegroups.com


Dear Expert,
We are facing some problem consisting of some little weld cracks that appreared after PWHT.
These cracks are within joint between thé LPG Sphere (4000 Cum) and its settling skirt.

As i remembrer in ASME VIII, repair of thèse cracks Could be done and only local HT Will be required.
Our client confirmés that as per CODAP 2005, thé HT after repair should concern thé concerned joint in all the sphere circonference, which is a real big problem.

Please share your expérience in similar cases.

BR


Sent from my ThinkPad S230u



--
Meilleures salutations

MOKRANI Lassaad
Consultant Civil Engineer
Tunisia
00216 20 649 755
http://www.linkedin.com/pub/lassaad-mokrani/16/364/907


















P     Pensez environnement! N'imprimez ce mail que si c'est vraiment nécessaire
Please consider your environmental responsibility before printing this e-mail


This e-mail is confidential and it is intended only for the addressees. Any
review, dissemination, distribution, or copying of this message by persons
or entities other than the intended recipient is prohibited. If you have
received this e-mail in error, kindly notify us immediately by telephone or
e-mail and delete the message from your system. The sender does not accept
liability for any errors or omissions in the contents of this message which
may arise as a result of the e-mail transmission

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...