Dear Sandeep:

A few things happen with Stress Relief:

  1. residual stress makes every thing brittle. Metals are more tough when they are not in tension and weldments always have residual stress at levels close to yield point.
  2. SR will temper the microstructure. This tempering like quench & temper steels, have a possitive effect on toughness and reduces brittleness.
  3. SR helps residual austenite transform to ferrite. This improves toughness.
  4. SR will reduce Hydrogen level in the weldment.

Hope you get the idea...

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.kondori@petroyada.com
+98-2123592322
+98-9132150320



On Sun, Jun 30, 2013 at 3:24 PM, sandeep monody <smv.monody@gmail.com> wrote:
Dear sir

Thanks for your reply and I understand your explanations.

But now please clarify how does the brittleness changes after pwht?

I think no physical properties will change without change in chemical properties.


Sandeep.m.v

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm

The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...