Skip to main content

RE: [MW:17991] SCC of Stainless Steel in H2S service

Avinash,
 
Traditionally offshore  oil and gas production involves both sour (High H2S) and chloride environment (due to high salinity of sea water). Sour service especially in the presence of wet H2S , generates tremendous amount of "nascent hydrogen" which charges on to the materials used for construction.
 
MR -0175 explains in great length what're the consequences of this "nascent hydrogen charging " which causes various forms of hydrogen induced cracking. Hardness control, heat treatment, cleanliness , good welding practices are required to mitigate this.
 
As austenitic S.S is prone to chloride SCC, one has to be very careful about selection of these alloys for sour service. 
 
Table A-2 in  ANSI/NACE MR0175/ISO 15156-3:2009 addresses these  concerns related to both"Chloride Conc" and "H2S partial pressure" and " Max recommended Design Temperature(60 to 149 Deg C)".
 
Note temperature is very critical to avoid Chloride SAC. The 300 series alloy/s  commonly  accepted for sour service is SS 316/316L.
 
The attached document gives a good description of  sulfide stress cracking.
 
Thanks
 
 
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Shomenath Bagchi
Sent: Thursday, June 20, 2013 5:23 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:17986] SCC of Stainless Steel in H2S service

H2S is a worse corroding medium for SS than chloride. SCC depends both on corrosive medium and stress.
For details, please check on SCC in Metals Handbook or net.


From: "avinash.araj@gmail.com" <avinash.araj@gmail.com>
To: materials-welding@googlegroups.com
Cc: Shomenath Bagchi <snbagchi@ymail.com>; snbagchi@ymail.com
Sent: Thursday, June 20, 2013 1:47 PM
Subject: Re: [MW:17985] SCC of Stainless Steel in H2S service

Dear Sir,
 
Thanks for your reply.
I agree that  SCC (Stress Corrosion cracking) damage in Stainless steel is multiplied because of STRESS.
 
But my query here is that this SCC effect (because of chloride and stress) is even more damaging in Presence of H2S (sour service).
 
Can you please explain this phenomenon?
 
Following is an extract from NACE MR-0175/ISO-15156 "
"stress corrosion cracking SCC
cracking of metal involving anodic processes of localized corrosion and tensile stress (residual and/or applied) in the presence of water and H2S.
NOTE Chlorides and/or oxidants and elevated temperature can increase the susceptibility of metals to this mechanism of attack."Regards
Avinash Araj
 
On Thursday, June 20, 2013 10:30:31 AM UTC+5:30, Shomenath Bagchi wrote:
Simply put, applied stress (stress energy stored in material) aids corrosion and expand small fissures in cracks.
 
 

From: "avinas...@gmail.com" <avinas...@gmail.com>
Sent: Wednesday, June 19, 2013 4:28 PM
Subject: [MW:17980] SCC of Stainless Steel in H2S service
 
 
Dear All,
 
I require your expert guidance on the below matter.
 
As we all know SS matl is prone to SCC (Stress corrosion cracking) in presence of Chlorides.
Now, as per various articles on the net, when this matl is additionally subjected to wet H2S service, the damage due to SCC is increased significantly.
 
So susceptibility of SS to SCC, is more in wet H2S /Sour service.
 
Can anyone put a light on this subject, as to why/how this happens?
 
Regards
Avinash
--
To post to this group, send email to material...@ googlegroups.com
To unsubscribe from this group, send email to materials-weld...@ googlegroups.com
For more options, visit this group's bolg at http://materials-welding. blogspot.com/
  
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@ googlegroups.com.
  
  
 
 
 
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...