Apart from knowing about polarity selection like,

DC EN (Electrode Negative) / DC -ve  (electrode Holder connected to Negative side of the pole)  /
DC Straight Polarity (Electrode / Holder connected  Straight  to Negative side of the pole  ---
are all same. Electrode coating / binder used to bond the chemicals makes this choice possible.

All Rutile coated  type & added and with Potassium silicate as a binder works well with DCEN  only ..
example - E6013, E7013 or all electrodes ( EXXX3) ending with numerical no.3  

All Rutile coated - iron powder type & added with Titania  also works well with DC EN. only.
example - E7014, E7024 or all electrodes ( EXXX4) ending with numerical no 4  

------------

DC EP (Electrode Positive) / DC +ve  (electrode Holder connected to Positive side of the pole)  /
DC Reverse Polarity (Electrode / Holder Reversed from Straight  to Positive side of the pole  ---
are all same. Here also electrode coating / binder used to bond the chemicals makes this choice possible.

All Cellulose coated  type & added  with Sodium silicate as a binder works with DCEP  only.
example - E6010, E7010 or all electrodes ( EXXX0) ending with numerical no..0  

All  basic / low hydrogen coated type  & added with Sodium silicate as a binder works with DC EP.
example - E7015, E 9015 or all electrodes ( EXXX5) ending with numerical no.5  

All  basic / low hydrogen coated type  & added with Potassium silicate as a binder works with DC EP.
example - E7016, E 10016 or all electrodes ( EXXX6) ending with numerical no.6  

All basic / low hydrogen coated - iron powder type & added with Potassium  silicate as a binder also works
well with DC EP.     example - E7018, E9018 or all electrodes ( EXXX8) ending with numerical no 8.

In SS electrode category, all types of electrodes including E 308 -17 / E316 -17  or  E308 -16 / 316 -16 (Rutile coated)
works  with DCEP as well as AC also.

All types of SS electrodes including E 308 -15 / E316 -15 ( basic coated) works with DCEP only..

Trust above info. will be  of help to you.

Sridhar.

 

----- Forwarded Message -----
From: Sinadurai Sripadmanaban <snaban@gmail.com>
To: materials-welding@googlegroups.com
Sent: Thursday, 20 June 2013 6:44 PM
Subject: Re: [MW:17989] RE: 17965] Clarification on Current and Polarity Abbreviations

Please give a list of metals & other items including stainless steel for which +ve to be connected to electrode as well as for which metal -ve to be connected to electrode.
Sinnadurai.S


On Tue, Jun 18, 2013 at 11:12 PM, John Henning <jhenning@deltak.com> wrote:
As I understand from welding people even older than I;  in the beginning days of welding, DC welding was performed with direct current power supplies with the electrode being the negative pole.  As welding progressed some, people found that SMAW welding with cellulosic  coverings "ran" better with the electrode positive or "reverse" polarity.  This may be a true story or it may just be propagated mythology.  At any rate -
 
For basic welding you can have an alternating current (AC) power supply or a direct current (DC) power supply.  With DC you have two options:   (1) electrode as the negative pole and the work piece the positive pole or (2) electrode as the positive pole and  the work as the negative pole.
 
DC straight polarity (DCSP) is the same as DC electrode negative (DCEN).  There may also be non-standard designations such as DC-, or DC-VE.
 
DC reverse polarity (DCRP) is the same as DC electrode positive (DCEP).  Or similar to above, non-standard DC+, or DC+VE.
 
Hope this helps.
 
John A. Henning
Welding & Materials
 
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Anban
Sent: Tuesday, June 18, 2013 4:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:17965] Clarification on Current and Polarity Abbreviations
 

Dear Experts
Pls enlighten me if thse abbr. are same and explain the correlation and difference


1 -  DCEP x DC+VE  x DCSP
2 -  DCEN x DC-VE x DCRP

DCEP - Direct Curent Electrode Positive
DCSP - Direct Current Straight Polarity
DCRP - Direct Current Reverse Polarity

Appreciation in advance
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...