Skip to main content

TIG for titanium tubing-Success hinges on filler metal selection, cleanness, gas coverage

TPJ - The Tube & Pipe JournalĀ®

TIG for titanium tubing

Success hinges on filler metal selection, cleanness, gas coverage

By Jack Fulcer
October 28, 2008

Although titanium has a reputation for being difficult to weld, it doesn’t have to be problematic. Paying close attention to filler metal selection, cleanness, and use of the shielding gas are three steps to successful GTAW on titanium tube and pipe.

TIG Titanium Tubing

Titanium is 45 percent lighter than steel, 60 percent heavier than aluminum, and more than three times stronger than either of them. While it is much more expensive than many other metals, it has greater corrosion resistance, lower life-cycle costs, longer service life, and drastically lower maintenance and repair costs than most. Common applications for titanium include military, aerospace, marine, chemical, power generation, oil and gas extraction, and medical devices.

Titanium is a reactive metal that interacts readily with oxygen, making it prone to oxidization and contamination, and making it difficult to weld. However, meticulous preparation, a steady hand, and lots of practice lead to successful welds.

This article focuses on gas tungsten arc welding (GTAW, also known as TIG welding, or tungsten inert gas welding) on titanium tube and pipe using ASTM Grade 5 titanium (Ti6Al4V) as a reference.

Cleanness Is Critical

Welding titanium tubing requires extreme cleanness—the base metal, filler metal, and welding environment must be immaculate. Contamination by natural body oils, oils from the forming and drawing process, shop dust, paint, dirt, cutting fluids, and lubricants all can lead to embrittlement and weld failure.

Start by cleaning the work area and ridding it of any debris, and be certain to choose a place with minimal airflow so as not to disturb the shielding gas during welding. Next degrease both the filler rod and the base metal: Wear nitrile gloves dedicated to this purpose to prevent body oils from rubbing off on these items. Then apply methyl ethyl ketone (MEK) to a clean, lint-free cloth and wipe the titanium to remove any remaining surface contamination. At this point place the filler rod into an airtight container to prevent further contamination.

Before welding, remove the oxide scale, which forms when the titanium reacts with oxygen, from the surface of the tubing. This oxide layer provides titanium with its notable corrosion resistance. Still, it must be removed before welding because it melts at a higher temperature than titanium and can enter the molten weld pool to create inclusions that weaken the weld.

Either a die grinder with a carbide deburring tool or a carbide file—both dedicated to titanium—works best to remove the oxide layer from the weld joint. Steel wool and abrasives are not recommended because they can cause contamination. Remember to use a low grinding speed to prevent excessive heat. Wipe the joint once more with MEK or acetone-soaked cloth after the oxide layer has been ground away. Wait for the solvent to fully evaporate before striking an arc, because some solvents have low flash points.

A Perfect Fit(up)

Joint fit-up is arguably more important on titanium tubing than on any other metal tubing because it is critical to prevent oxygen from entering the weld. The joint should be square (do not create a V-notch), which helps minimize the amount of heat and weld metal needed to fill the joint; this in turn lowers the chance of burn-through and contamination.

Clamp the pieces into a positioner or on a workstation to make sure the two ends are butted together as tightly and accurately as possible.

You do not need to preheat most thin-wall titanium tubing and pipe. However, consult with your welding equipment supplier if you plan to weld titanium more than 1⁄8 inch thick, because some preheat and postheat may be beneficial.

The Importance of Shielding Gas Coverage

Pure argon is recommended for welding titanium because of its high purity and low moisture content. A 75/25 mixture of argon/helium may be used to improve stability and increase penetration only when specified.

The American Welding Society (AWS) recommends measuring welding gas purity to make sure it meets the standards set for each application. Typical specifications suggest that shielding gas be at least 99.995 percent pure with no more than 20 parts per million (PPM) of oxygen and a dew point greater than -76 degrees F. Other applications require a 99.999 percent pure flow of argon.

Outfitting your welding torch with a trailing shield is critical—otherwise the risk of oxygen contamination rises, and with it the potential for cracking. Some welders fabricate their own trailing shields, although many styles are available for purchase. Trailing shields conform to the shape of the tube and follow the GTAW torch around the pipe. The shields provide an extra protection of argon over the weld after the torch and its argon flow have passed. Setting the torch and trailing shield gas flow at 20 cubic feet per hour (CFH) provides the best coverage.

Purging, a process that eliminates the oxygen contained within the pipe, also

is required when welding titanium tubing. This process can be completed with any kind of purge dam: water-soluble dams, rubber gaskets, specialty tape, or inflatable bladders. Argon flows into the dammed area to replace the oxygen contained within the tubing. Allow the argon to flow long enough to replace the oxygen 10 times over to ensure the purest welding environment.

Always use a clean, nonporous plastic hose to transport the shielding gas to the torch, trailing shield, and purge. Do not use rubber hose; rubber is porous and absorbs oxygen that could contaminate the weld.

Filler Metal Selection

Use a filler metal when welding titanium tubing thicker than 0.010 in. (see Figure 1). Typically, you should match the filler metal to the grade of titanium being welded—it should be an exact match. Some applications allow exceptions, such as a filler metal with a lower yield strength than the base metal to improve ductility. Any variation, however, should be carefully tested and investigated to make sure it meets process demands and specifications.

Recommended Titanium Filler Metal Alloys

Base Filler

AWS A5.16 ERTi-2

AWS A5.16 ERTi-2

AWS A5.16 ERTi-3

AWS A5.16 ERTi-5

AWS A5.16 ERTi-9 and ERTi-9ELI

AWS A.16 ERTi-23

Grade 1 (CP-1
or commercially
pure)

X

 

 

 

 

 

Grade 2 (CP-2)

X

X

 

 

 

 

Grade 3 (CP-3)

 

 

 

 

 

 

Grade 9
(Ti3A12.5V)

 

 

X

 

X

 

Grade 5
(Ti6A14V)

 

 

 

X

 

X

Grade 23
(Ti6A14V ELI)
(extra-low
interstitial)

 

 

 

 

 

X

Figure 1

Picking the Right Torch and Consumables

GTAW gives the welder more control over heat input and the puddle than any other welding process. A GTAW inverter with high-frequency arc starts, remote amperage control capabilities, a postflow timer, and an output of at least 250 amps, will weld titanium nicely.

Always set the machine's polarity to direct current electrode negative (DCEN). DCEN offers deeper penetration and a narrower bead in comparison to direct current electrode positive (DCEP).

Match the inverter with either an air- or water-cooled torch. An air-cooled torch provides good performance if you're welding below 150 amps and it costs less than a water-cooled torch. On the other hand, a water-cooled torch is smaller, more maneuverable, and permits welding at higher amperages for extended periods, although most welds on titanium are short and created at output levels below 150 amps.

Use a 2 percent ceriated tungsten electrode ground to a point and matched to the welding current as follows:

Ā·  Up to 90 amps: 1⁄16 in. or smaller

Ā·  90 - 200 amps: 3⁄32 in.

Ā·  More than 200 amps: 1⁄8 in.

Use a gas lens to distribute the shielding gas evenly and to create a smooth gas flow over the weld puddle.

Strike an Arc and Get to Work

First, cut off the end of the filler rod to expose a pure, contaminant-free point to start the weld. Start the argon gas flowing for a few seconds before striking the arc to ensure the weld area is fully covered.

Use the inverter's high-frequency arc-starting feature to strike an arc. Torch angles, torch speed, and filler wire angles similar to those used in welding stainless steel provide optimal conditions for welding titanium tubing.

It is fairly easy to create the weld puddle with titanium, but it may not move easily. Pushing the weld puddle along with the arc and the filler rod generally provides the best results, but you must keep the filler rod within the shielding gas envelope while welding. It's also important to minimize heat input because excessive heat can crack the weld. Use a dab technique (at a steady travel speed) with the filler metal instead of leaving the rod in the puddle at all times.

Once you are finished with the weld, allow 20 to 25 seconds of postflow to protect the seam as it cools down below the 800-degree-F threshold. This is the point at which oxygen no longer reacts with titanium. Some welding codes may require postflow until the temperature drops below 500 degrees F, so always follow the written procedure.

Titanium offers the benefit of showing its true colors once the weld is finished. The final color of the weld joint indicates how well the shielding gas protected the weld from contaminants and how thick the oxide layer is (see Figure 2). In addition to visual inspection, dye penetrant inspection, hardness testing, X-ray, ultrasonic, and destructive tests determine the quality of titanium welds.

Color Acceptance Criteria

Weld Color

Quality Indication

Bright Silver

Acceptablea

Silver

Acceptablea

Light Straw

Acceptablea

Dark Straw

Acceptablea

Bronze

Acceptablea

Brown

Acceptablea

Violet

Unacceptableb,c

Dark Blue

Unacceptableb,c

Light Blue

Unacceptableb,c

Green

Unacceptableb,c

Gray

Unacceptable

White

Unacceptable

Figure 2

 

 

 

 

Ā·                           

 

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...