Re: [MW:35834] Re: Hardness range for CS

Dear Mohammed, Thank you for your response. We're facing another significant issue. Most of our carbon steel Procedure Qualification Records covering groups G1-G2, G1-G3 & G2-G3, G3-G3 with various process combinations are showing an unacceptable hardness range (260–325 HV) in the Heat-Affected Zone. Our maximum acceptable hardness limit is 250 HV. We've used different testing agencies, yet the results remain consistently high. Regards, Saurabh On Fri, 17 Oct 2025 at 8:26 AM, Mohmmed Dudhiyawala < mdudhiya007@gmail.com > wrote: Dear Saurabh, Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d. Refer Table A.14. From Temp<149°C, Inconel 625 can be used for all conditions, stipulated in table. Hardness to be limited to 40 HRC max. (392 HV). Regards, Mohammed On Tuesday, August 19, 2025 at 7:47:46 AM UTC+5:30 Saurabh Jain wrote: Dear experts. I am currently in the process of qualifying a PQR for API 5L X65 + A350 LF6. ...

[MW:35832] Re: Hardness range for CS+ Alloy0625 clad welding

Dear Saurabh, Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d. Refer Table A.14. From Temp<149°C, Inconel 625 can be used for all conditions, stipulated in table. Hardness to be limited to 40 HRC max. (392 HV). Regards, Mohammed On Tuesday, August 19, 2025 at 7:47:46 AM UTC+5:30 Saurabh Jain wrote: Dear experts. I am currently in the process of qualifying a PQR for API 5L X65 + A350 LF6. Both material consists of a base metal with alloy 0625 cladding. Welding process: GTAW+SMAW During the mechanical testing, I witnessed the following hardness values: Clad material: 300 to 390 HV Weld metal: 280 to 350 HV This is for Aramco project, so I referred their standard 01-SAMSS-044, and it specifies that I must refer to NACE MR0175/ISO 15156 for hardness acceptance criteria, particularly for the clad. I have reviewed the standard but cannot find a specific acceptable hardness range. I also checked Aramco's W-11/W-12 and W-16 standards but was unable ...

[MW:35832] 625 Weld Overlay on SA516 Gr70 plate in 3G position

Hi Everyone, We have encountered as PQR for Inconel-625 WOL on SA516 Grade 70 Normalized plate in 3G position. Two Anomalies were observed:  1. After PWHT of 120 mins, Hardness in base metal dropped from average 164 HV to average 108 HV! Has anyone observed such a drop in hardness? Is it possible?  2. 625 WOL is done using SMAW electrode from Special Metals, the Nickel content as per consumable TC is 65%. While in WOL chemistry, 1.5mm from Top, Nickel % came around 68%. 3% Higher!! Is this possible, in any case? Thanks in advance from your expert views. Regards, Mohammed Dudhiyawala, IWE -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.googl...

[MW:35835] filler Rod Inconel 693 (ERNiCrFeAl-1)

Dear All, Can someone advise where I can find the filler rod for the specification of ERNiCrFeAl-1. AWS.A 5.14 I have check to special metal however they are not producing any more for this filler.  Thank you for your information guys.  Regards MK Noor  -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/fff02307-7fa0-4685-b823-ec205ea0d8e3n%40googlegroups.com .

Re: [MW:35836] Re: Hardness range for CS

Hi,  What was your heat input reading? Thank you & Stay Safe!   KAVIN MURUGAM +60126159644 On Fri, Oct 17, 2025 at 2:18 PM Saurabh Jain < ensaurabh@gmail.com > wrote: Dear Mohammed, Thank you for your response. We're facing another significant issue. Most of our carbon steel Procedure Qualification Records covering groups G1-G2, G1-G3 & G2-G3, G3-G3 with various process combinations are showing an unacceptable hardness range (260–325 HV) in the Heat-Affected Zone. Our maximum acceptable hardness limit is 250 HV. We've used different testing agencies, yet the results remain consistently high. Regards, Saurabh On Fri, 17 Oct 2025 at 8:26 AM, Mohmmed Dudhiyawala < mdudhiya007@gmail.com > wrote: Dear Saurabh, Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d. Refer Table A.14. From Temp<149°C, Inconel 625 can be used for all conditions, stipulated in table. Hardness to be limited to 40 HRC max. (392 HV). Reg...

Re: [MW:35837] Re: Hardness range for CS

0.60 to 2.22 On Fri, 17 Oct 2025 at 4:06 PM, kavin murugam < kavin.murugam@gmail.com > wrote: Hi,  What was your heat input reading? Thank you & Stay Safe!   KAVIN MURUGAM +60126159644 On Fri, Oct 17, 2025 at 2:18 PM Saurabh Jain < ensaurabh@gmail.com > wrote: Dear Mohammed, Thank you for your response. We're facing another significant issue. Most of our carbon steel Procedure Qualification Records covering groups G1-G2, G1-G3 & G2-G3, G3-G3 with various process combinations are showing an unacceptable hardness range (260–325 HV) in the Heat-Affected Zone. Our maximum acceptable hardness limit is 250 HV. We've used different testing agencies, yet the results remain consistently high. Regards, Saurabh On Fri, 17 Oct 2025 at 8:26 AM, Mohmmed Dudhiyawala < mdudhiya007@gmail.com > wrote: Dear Saurabh, Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d. Refer Table A.14. From Temp<149°C, Inconel 625 can ...

Re: [MW:35838] Re: Hardness range for CS

Is this PQR is with PWHT ? On Fri, 17 Oct 2025 at 11:48 AM, Saurabh Jain < ensaurabh@gmail.com > wrote: Dear Mohammed, Thank you for your response. We're facing another significant issue. Most of our carbon steel Procedure Qualification Records covering groups G1-G2, G1-G3 & G2-G3, G3-G3 with various process combinations are showing an unacceptable hardness range (260–325 HV) in the Heat-Affected Zone. Our maximum acceptable hardness limit is 250 HV. We've used different testing agencies, yet the results remain consistently high. Regards, Saurabh On Fri, 17 Oct 2025 at 8:26 AM, Mohmmed Dudhiyawala < mdudhiya007@gmail.com > wrote: Dear Saurabh, Refer Table A.12 of NACE MR0175/ISO 15156, where Inconel 625 is designated as Type 4d. Refer Table A.14. From Temp<149°C, Inconel 625 can be used for all conditions, stipulated in table. Hardness to be limited to 40 HRC max. (392 HV). Regards, Mohammed On Tuesday, August 19, 2025 at 7:47:46 AM UTC+5:30 S...