Re: [MW:35926] Duplex WPS for Super Duplex

Yes you are right, shielding gas also one of the essential variables. Along with P number and F number other parameters also we have to consider before choosing WPS.


On Mon, 15 Dec 2025, 7:35 pm Anandhapadmanabha pillaim, <anandhapadmanabhapillaim1997@gmail.com> wrote:
As per ASME Section IX, the use of SDSS filler wire is permitted even when impact testing is not specified or required, provided the essential variables are met.

However, beyond the code requirements, from a metallurgical and performance standpoint, DSS and SDSS differ significantly in their ferrite-austenite phase balance requirements. Achieving the correct phase balance is critical and is strongly influenced by welding heat input. SDSS, in particular, has a higher PREN (Pitting Resistance Equivalent Number) requirement compared to DSS.

To achieve the required PREN and phase balance in SDSS weld metal, nitrogen is commonly added to the shielding and backing gas. Nitrogen is a strong austenite stabilizer and also contributes to an increase in PREN, thereby improving corrosion resistance.

If a WPS is qualified for DSS using pure argon as the shielding gas, and it is later proposed to use an argon–nitrogen mixture (for Eg: Ar + 2% N₂) for SDSS welding, this change would require requalification of the PQR. This is because the addition of nitrogen significantly affects weld metal chemistry, phase balance, and mechanical and corrosion properties, making it a metallurgically significant change even if not explicitly listed as an essential variable in all cases.

That said, if the required mechanical properties, corrosion resistance, and phase balance are successfully achieved using the same gas composition qualified for DSS (i.e., pure argon), ASME Section IX permits its use, as long as all applicable essential and supplementary essential variables remain within the qualified range.

On Mon, 15 Dec 2025, 5:29 pm Alex Kumar Antony, <alexkantony@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/ee5dcbf4-b6cb-4421-8338-04e109d45b15n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJ90KGR%2BWjiOTHjPf4mNLed34QHj4QP3_KD%2BzfeckX20tFydUA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAEabyKmcprT%3DtXzC5si2hWGpBe7j5Q43pvSYtw_mrTJV7_WY%2BA%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...