Re: [MW:35926] Duplex WPS for Super Duplex

Code-Based Explanation (ASME Section IX)

1. Base Material Grouping – P-Numbers

ASME Section IX groups materials by P-Numbers to control essential variables.

  • Duplex Stainless Steels (e.g., UNS S31803 / S32205)
    P-No. 10H

  • Super Duplex Stainless Steels (e.g., UNS S32750 / S32760)
    P-No. 10I

📌 Since P-No. 10H ≠ P-No. 10I, they are treated as different base material groups.


2. Essential Variable for Base Materials

ASME Section IX clearly states:

QW-403.11
A change from one P-Number to another P-Number is an essential variable and requires requalification of the WPS.

✅ Therefore:

  • A WPS qualified on Duplex (P-No. 10H)

  • Cannot be used for Super Duplex (P-No. 10I)

  • Without a new PQR covering P-No. 10I


3. Mechanical and Metallurgical Differences (Supporting Rationale)

Although not strictly required by code, this reinforces why the rule exists:

  • Super Duplex has:

    • Higher PREN

    • Higher yield and tensile strength

    • Tighter control on heat input, interpass temperature, and ferrite/austenite balance

  • Welding Super Duplex with a Duplex-qualified WPS risks:

    • Loss of corrosion resistance

    • Sigma phase formation

    • Improper phase balance

Codes intentionally separate these alloys due to these risks.


4. Filler Metal Consideration (Additional Control)

Even if a Super Duplex filler metal is used, the limitation still applies, because:

QW-404 (Filler Metal Essential Variables)
Filler metal control does not override base material P-Number limitations.


Final Conclusion (Code-Compliant Answer)

A Duplex WPS cannot be used for Super Duplex welding.

ASME Section IX requires requalification, because:

  • Duplex = P-No. 10H

  • Super Duplex = P-No. 10I

  • Change in P-Number is an essential variable per QW-403.11


On Mon, Dec 15, 2025 at 9:28 AM Alex Kumar Antony <alexkantony@gmail.com> wrote:
Can we use Duplex WPS for Super Duplex, kindly quote with the help of code
Thanks

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/ee5dcbf4-b6cb-4421-8338-04e109d45b15n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAHXTn13GP75Hk7hisbt4yD5v5brzSvKEUfseobmjDxGf6JqYNQ%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...