Re: [MW:34431] Corrosion Test Fail For Duplex Steel

Just to add a portion from API RP582.

Inline image


Thanks & Regards

J.Gerald Jayakumar




On Wednesday, 19 July, 2023 at 09:08:39 am IST, Babur Khan <mbabur.bwp@gmail.com> wrote:


Greetings,
In pas we faces same issue and after that we get recommendations from test laboratories to use mixture gases for shielding and purging.
Argon + 2% Nitrogen mixer with ER2594 filler wire.a

 Babur Khan Lashari 

Sent from my iPhone

On 18 Jul 2023, at 2:16 PM, Ashish Chacko <iamashleo007@gmail.com> wrote:

Backimh and shieldimg gas was argon grade 4.7 b ( 99.997%)

On Tuesday, 18 July 2023 at 11:10:50 UTC+3 Vishwas Keskar wrote:
What was the backing and shielding gas ?

Sent from my iPhone

On 18-Jul-2023, at 10:56 AM, Ashish Chacko <iamash...@gmail.com> wrote:



I am currently working on developing a Procedure Qualification Record (PQR) for Duplex Steel. In the process, I conducted welding using the base material SA 790 (UNS:32205) and utilized two different filler wires: ER-2594 and ER-Nicr-Mo-14 for different coupons. Size of the coupon 6" Thick:10.97 mm.

However, I encountered a concern during the corrosion testing phase, as per ASTM A923-03 standards. Both test materials failed the corrosion test. I'm seeking guidance from the experts in this group to understand the possible reasons for the failure and to explore potential solutions or alternative approaches.

If anyone has experience with similar issues or insights into the matter, I would greatly appreciate your assistance.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8de07ffa-c770-4e90-ab75-f83b3089d3b0n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/7068eff6-31d3-4d90-b0a0-84266c712e75n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/E4B944BA-2609-43FF-B9E5-6E01105B2565%40gmail.com
.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...