Dear , 
As follow saudi aramco standard and procedure ,  saes-a-004, saes-l-150, following are my observations

Water used for hydro testing of stainless steel piping systems shall have chloride content value less than 50ppm, and PH value should be 7.5, ±.5.

Water used for any part of the hydro testing or subsequent lay-up shall have a sulfate reducing bacteria (SRB) count of 10³ per ml or less

When the equipment contact time with hydrotest water may exceed 14 days, an approved oxygen scavenger shall be added to the hydrostatic test water.

For stainless-steel piping, the duration of the hydro testing (using water with less than 50 ppm of chlorides), flushing and draining-drying sequence shall be kept as short as possible, in order to reduce the possibility of chloride attack. Water testing certificate will be made available for each hydro test

regards 

Dhaneesh 



On Fri, Sep 18, 2020 at 5:48 PM Manish Kumar <mkmkr431@gmail.com> wrote:
Sir,
How much Ph value is required for Hydrotest in Stainless steel piping and equipment.Please advise as per reference of relevant standard & Code.

On Fri 18 Sep, 2020, 5:38 PM Vishwas Keskar, <vvkeskar123@gmail.com> wrote:
use water with Chloride content less than
 25 ppm
use potable water
do water analysis 

On Fri, 18 Sep 2020, 15:38 Manish Kumar, <mkmkr431@gmail.com> wrote:
Dear Sir,
I want to know that which type of water is used for Hydrotest in stainless steel piping and equipment. Please advise as per relevant code and standard.




--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k7ZV%2B%3DrkXu%3DSdnx2zeGsMf83xjjA%2B4-CLvDzZ1TBuuBfg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3P9%2Bfx%3DaawdsnsTePqFj7W09SMCfy5-tLnkfZ8OS1wHMw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHfQ4k6B4ZuqjvGU7OpupRWFSxN55f3uP4Tw4DssquqyoVUKxw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHZhELcmHCbdtCsGOkHKh0DiNXtvag%2B5sArsT7BwB7JGMpREVA%40mail.gmail.com.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...