Skip to main content

Re: [MW:27745] impact testing of welding consumable , ASME VIII Div 1

Hi Ramesh,

Your interpretation is correct as specified in below mail.

Impact test exempted for PQR qualification i.e. weld and HAZ, provided welding filler metal as specified in SFA specification shall confirm CVN test at MDMT or Colder temperature.

In this case filler metal is specified with -30 Deg. C CVN test and MDMT is -46 Deg. C and hence welding filler metal shall be tested at -46 Deg. C. This requirement shall be included in the PO stage itself so that filler metal manufacturer shall take care of impact test at -46 Deg. C (with minor medication of elements to improve toughness). Do not procure and test at -46 Deg. C with may pass for some batch and however it shall be ensured by the filler metal manufacturer.

Hope it is clear.

L. Prabhu kumar
Ph. no.+91 9003010978/ +968 95202761.


From: Ramesh <rameshkannandevaraj@gmail.com>
Sent: Wed, 18 Apr 2018 12:38:00
To: materials-welding@googlegroups.com
Subject: Re: [MW:27723] impact testing of welding consumable , ASME VIII Div 1
 
Hi

 

My understanding about UCS-67(a)(3) as below

 

Your PQR impact testing may be exempted provided

 1 .Your Filler metal shall be classified by their manufacturer through impact testing at a temperature not warmer than the MDMT 

But, In your case, TC has been reported as -30 Deg C.  You can use these batch consumables up to -30 Deg C MDMT without impact testing ( Not for -45 Deg C MDMT) hence exemption is NOT applicable for you.

 2. Additional testing beyond the scope of the SFA specification may be performed by the filler metal and/or flux manufacturer to expand their classification for a broader range of temperatures  - which is  self-explanatory - you need to have TC for -45 Deg C tested temperature

 Also I have attached some relevant interpretation details for your reference

Official web page for all interpretation available in link below. You may find many interpretation available related to this topic.

<https://cstools.asme.org/Interpretation/SearchInterpretation.cfm>

 

 

 

 

 

 

 

 
On Tue, Apr 17, 2018 at 12:16 PM, gigi <anhtrangnghieng@gmail.com> wrote:

Dear Gent,

 

Non- impact tested WPS was used for some weld joint. Question :

·         If welding consumable ER70S-G have been impact tested at –30°C . As per para. UCS-67(a)(3), additional testing ( Impact test ) at –45°C is a requirement when WPS ( No impact test ) used ?

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ramesh
Sent: Tuesday, April 17, 2018 12:22 PM
To: materials-welding@googlegroups.com
Subject: Re: [MW:27708] impact testing of welding consumable , ASME VIII Div 1

 

Hi

You mean , already welded using non-impact tested WPS/PQR ?

 

Your PQR should have been qualified with impact testing, then only para.UCS-67(a) is applicable for u

Seems, your consumable supplier supplied ER 70S-G with guaranteed values up to minus 30 deg C only, which may not suitable for your MDMT, unless tested.

Ask supplier to replace your consumable to meet your service requirements. 

 

As per ASME BPVC.II.C-2017 SFA-5.18/SFA-5.18M,

Impact testing requirements should have been agreed before you place order, since no requirements as per code

 

​ 

 

  Either case you should have qualified WPS/PQR to meet your service requirements .

 

 

 

 

On Tue, Apr 17, 2018 at 9:25 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:

yes

 

THANKS & BEST REGARDS,

KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Mon, Apr 16, 2018 at 7:16 PM, Vanchinath S.A. <vanchinaths@gmail.com> wrote:

You have to qualify WPS with impact test at mdmt.

 

On Mon, 16 Apr 2018, 19:10 gigi, <anhtrangnghieng@gmail.com> wrote:

Dear Experts,

 

Please help me to clarify issue as below:

 

Solid rod ER70S-G have been used for weld joints of HP Flare KO Drum by using WPS V02 (GTAW/SMAW – Impact test is not applied). Certificate of welding consumable ER70S-G indicates that impact test temperature is –30°C. Minimum design metal temperature (MDMT) of HP Flare KO Drum is –45°C. Material of HP Flare KO Drum is SA-516 Gr60 normalized.

In accordance with para.UCS-67(a)(3) ASME BPVC.VIII.1-2017 , is it a requirement to perform impact test at –45°C for welding consumable ER70S-G?

 

Thanks

 

Gigi.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...