Wednesday, April 11, 2018

RE: [BULK]Re: [MW:27674] Stainless steel (SA 312 TP 316L) welding

Hi Prasad,

 

As explained previously by one of the forum members , ferrite to the extent of 3-6%(volumetric) or 3-6FN is required in the 316/316L welds to avoid hot cracking. Welding consumables are manufactured with the required composition chemistry to achieve this target.

 

However measurement of ferrite in the welds are  process/project requirement. All corrosive services involving 300 series alloys  calls for mandatory "Ferrite " control in  welds.

 

What's the operating service  involved in the design??

 

Thanks.

 

 

P.Goswami.P.Eng, IWE.

Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

 

Refer this IIW document for Better Understanding  on Ferrite in weld Metals.: IX-1695-92-(IIW-1166-92-IX-H-233-90)-Guidance-on-specifications-of-ferrite-in-stainless-steel-weld-metal

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: April 10, 2018 9:42 AM
To: materials-welding <materials-welding@googlegroups.com>
Subject: Re: [BULK]Re: [MW:27670] Stainless steel (SA 312 TP 316L) welding

 

Is it. If ferrite exceeds 8 or 10, what will happen and if it is less than 5 also

 

On Tue 10 Apr, 2018 6:23 pm Manoj Singh, <manoj.singh1178@gmail.com> wrote:

Hi, 

Thus sa312 tp 316 has moly therefore  moly is a promoter for ferrite and if there is excess fn in weld metal after it causes hardness and chances for brittle fracture increases that is why we need to check fn no. For 316

 

Thanks

 

On 10-Apr-2018 5:41 PM, "Kannayeram Gnanapandithan" <kgpandithan@gmail.com> wrote:

what is the reason for Hot cracking


THANKS & BEST REGARDS,

KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Tue, Apr 10, 2018 at 4:51 PM, Lu, Feng <luf@zachrygroup.com> wrote:

3 ~ 8% ferrite are required in the weld to prevent hot cracking

 

 

Zachry Group Logo

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: Tuesday, April 10, 2018 5:56 AM
To: materials-welding <
materials-welding@googlegroups.com>
Subject: [BULK]Re: [MW:27666] Stainless steel (SA 312 TP 316L) welding

 

what is the necessity for ferrite testing on 316L


THANKS & BEST REGARDS,

KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Tue, Apr 10, 2018 at 4:16 PM, Perumal Govindan <perumalgovindan@gmail.com> wrote:

Hi Prasad,

 

Ferrite testing is required when it is mentioned in the Client / Project Welding / Construction Specification.

 

 


With Kind Regards

 

P Govindan 

 

On Tue, Apr 10, 2018 at 11:24 AM, 'Shashank Vagal' via Materials & Welding <materials-welding@googlegroups.com> wrote:

NO

 

On Sunday, 8 April 2018 6:41 PM, Prasad Rode <purode333@gmail.com> wrote:

 

Dear sir,

I am going to do PQR for SA 312 TP 316L pipe to pipe of 6" and 7.11mm thickness.

I want to know that, i have to go for ferrite testing or not ?

If not, when it is essential to ferrite testing?

Regards
Prasad

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzLoctJUEMDdbzGqdXz0x9TjaAPfvUNCLPyWmBF72X02uczwD2w2oQr4w1WU83Qi9TlzHiZ7Q_m9togWnC_PifpMYG8Noh8ecDgt7Rz98rlzdDCP25FnmnS_fTsbYKEW23twpN4Bzour50n0apwtEnAxZYN9sAWmkWYerjHTOdoPgbEeCq6R1TaDdAKBlmlFHT4VODFg8bxr_Ky0_qRNkuh067eU3nfDwrJG-XJiwtMxynCYDVIZxQz1Fv74pM0X3HjGhj247CNngXDfoNc61SRf3RPhE2b34P5EiGja9P9JH-OsWp5vdlOZ_ev82Kyia9HdDn4kwpU9bD_Y/https%3A%2F%2Fwww.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at
https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5it9Jd9i_VDkw1AUQnt1B_8PvkK-5KPssj1ExOaVPMda4kh79O3-nwhzRckMK5PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ_fH7AtzprQyB5Qhj6i06A2Vtf5DvTMzg0taC8VPuylTiEN6kray-J6mSH7rD5orTEuXBUqWHY0XJTUW8BT0jVxHDa8Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc57xv9U6uF_6RuNqso_Kl_aOOPXwGTepm00WRQkCkB5IN5Bbp3nDX7n3z5YuRFaa6YDUiw3XQ4qTR9dNndOcf4Tb3V5CqSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8S-A/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit
https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D66SWirlI5SOn-YhcHDPOM5GhE6va5qKkPm_WjdJVCXM_Ev0AsJwnBggZ71lDFT-ump4X6eoB8B9kDI9imYMY1Egx6DHIGG4asTwbZiikNoMyLvIZn2hRyxaMgkPyo-CYZYNykefeET8HwTcUVqQBEPjS-MTu7OmiuqtRe_zpIH1qMlNrjblAuJjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKATiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd1OpQJkIAcpioyy8RD5qUkbwU9Ixs21FggLi3SNukHhJ3H-XBnX9R3JDCs3NfgZ3Olgx0BzW2UewBza6kNw3toz3lk6w6E/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzLoctJUEMDdbzGqdXz0x9TjaAPfvUNCLPyWmBF72X02uczwD2w2oQr4w1WU83Qi9TlzHiZ7Q_m9togWnC_PifpMYG8Noh8ecDgt7Rz98rlzdDCP25FnmnS_fTsbYKEW23twpN4Bzour50n0apwtEnAxZYN9sAWmkWYerjHTOdoPgbEeCq6R1TaDdAKBlmlFHT4VODFg8bxr_Ky0_qRNkuh067eU3nfDwrJG-XJiwtMxynCYDVIZxQz1Fv74pM0X3HjGhj247CNngXDfoNc61SRf3RPhE2b34P5EiGja9P9JH-OsWp5vdlOZ_ev82Kyia9HdDn4kwpU9bD_Y/https%3A%2F%2Fwww.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at
https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5it9Jd9i_VDkw1AUQnt1B_8PvkK-5KPssj1ExOaVPMda4kh79O3-nwhzRckMK5PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ_fH7AtzprQyB5Qhj6i06A2Vtf5DvTMzg0taC8VPuylTiEN6kray-J6mSH7rD5orTEuXBUqWHY0XJTUW8BT0jVxHDa8Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc57xv9U6uF_6RuNqso_Kl_aOOPXwGTepm00WRQkCkB5IN5Bbp3nDX7n3z5YuRFaa6YDUiw3XQ4qTR9dNndOcf4Tb3V5CqSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8S-A/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit
https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D66SWirlI5SOn-YhcHDPOM5GhE6va5qKkPm_WjdJVCXM_Ev0AsJwnBggZ71lDFT-ump4X6eoB8B9kDI9imYMY1Egx6DHIGG4asTwbZiikNoMyLvIZn2hRyxaMgkPyo-CYZYNykefeET8HwTcUVqQBEPjS-MTu7OmiuqtRe_zpIH1qMlNrjblAuJjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKATiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd1OpQJkIAcpioyy8RD5qUkbwU9Ixs21FggLi3SNukHhJ3H-XBnX9R3JDCs3NfgZ3Olgx0BzW2UewBza6kNw3toz3lk6w6E/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/15CdaQ7SqBttaMDjEgp4vyA1IIjLruZ4x02m8Ah9pYq6pSUFOK4-lHzhH7m7k9MIiS0unxn4qfOA70v59vOPWRGhNUrugmrLXvQ-X0WNEztRVJR8_iUnWuJL7ZngVRii6W0MHgWbayD58uOybu_o_WS7TXJfyWs-_7Fy3RGrk262seUpeYMyBOkVy6JjNeidtV2NikbqfRJ69VudWHlR7Pj1brCz_pmBZyqwiAvBxYfKg2Uu8IxnyW6iurEV6LnqgTLG1l95kaOCk5T8n2-t1_mZz0HXQowSp2KjuOD4Zb7ZnlfDrumTmHmUIr_DltelYqkudojkTlcFiSo_OS8RBn7ObjA0peImqj_vGZwZA27Y/https%3A%2F%2Fwww.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at
https://secure-web.cisco.com/1eRh-wf9X8OZeiSzdXfjjdBsreEz2vw6nypbfDtNb9gF9ga2ioNVBw6jsStnX7fBTJt1ESgLZHyRIrp3TXqnx28FIbMh1w8a3F8es4N0JYiKyPOeTKWWkEa9IIqUXxQ9P-Fjen_zx8xXb2UfxCrDNSatnz7YR3tcclkVDWvUGZWNSCxsHhWey9xdfpJ4q6yxf0Nphl2FTNTbt1uzeSbcMh-d1-maJnFMgDZv-W_0HKTlLLzJOpdn7ZZ0ojXZxwg2PSa2zxDZPuPyT49Qzb49J-Vn5b1A5yVIfU6jLSqX01kz5_VERtpsouoOvlyw_ExjdM_Rz3iU2CvSdWr3y5LILETR4FgI0PysBwPO2uVgBq70/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit
https://secure-web.cisco.com/1Gqw5l2Ew0NnLF9ocT7FiPSzoc7Xh5IXXL0ZUUCS2kBzZm-hHDlnrap_v-m_bjpNstyVad2i7EysoEtlOT4Te7ttRG-bQ3cta-FkTGYTXN1OiukqlCyELfHfF-mW95cAi6BWn-5VkwmqdM0MqNz5GayYxa_NlqaaeBiPR599qfT5pB4k82oN1UntSTlKDSO21R7GS84NHR7QhdtV8Jk8SnQeqMqgFiGqQ0xp6ZLe2oxwCz-6n-dTkyCYepQifCb4HSm2SkrJ5jla3kcWsKsa-GWg2J_u_WEMlfVJBriXkMRO9IQQ_2t-pZATcoezLzmb-EKYYb9PEqDsTxFrV5cu-lMxRMUoWqyFeOy10TFMtT90/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://secure-web.cisco.com/1Yekz4_Rk1j5eIKzWu3w3uOI4lY_995nOXaYoO2uO0NGqMQXH-ZV9VapwaVCb3IxXLLVZM8kjdu9fM7j1srk-jOXoitpI_KNfy6y596DmYrln7EAsMlF7l9hPmw01eSNbToT4y3p6Ek5qnqPiaII6IAqGJkGpUWHzaHjuP-_HJSX4av0Zg1TxLLPqX1jOpfkdDwcIKu_Ch0W90jC3sje2nKE3fvQdvq-EYXWuoP2PhBkY0GXwY1i2E3lGsFgt1uDo9QhRi4zd7373nAXJj-tQQipR7ApVH3skfaHyElP254ZeHlSze7RhOtIpzCm5v8VlQA1BgwYbg4CwFlK0wOolWVMJxCeqE-36laFK69SEhm4/https%3A%2F%2Fmaterials-welding.blogspot.com%2F
https://secure-web.cisco.com/1T4WuM8lkw7TepJTiGMw6aWBwIYmQBseyjuGtIJoulgjhLZ7EVw-eED0B1_ytTaqgwjwuKfJDC_-XzBITrF66Tr4OYoTqxRHrf5DQUoEx9xJI6uGsnT6T8rqf0HxLaPaKsrwqTgORJ2twvVMj_3SiNnhcIVIjbcKSjdNG1FQeNdUJGX4QZfXdCfYnvWOC5GWgApzenhyd2_29Hux1DpznKaRGakrq7I4wwOMAWVHQWE8OCzrYh7nIOtoZyGlAtn7VO4zhFjdXFddWZv8zbXOxkuYVLcN_iktDQ4QjpF2OH1olC3Yq6cQppUBAbQyMxLeGmFekICOzEPKI77xUxO43Tj1RtqibnEb207n4J3s-0nU/https%3A%2F%2Fwww.linkedin.com%2Fgroups%2F122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-welding+unsubscribe@googlegroups.com.
Visit this group at
https://secure-web.cisco.com/1Ngm51h-0qXokcX3NLuwji6oaxruW94TI5tEOmO1aty65EiLOKKAcQAr68FvwVf78F6_OtvN32tWU5Lo4oA7s1YkEXv0OHLp81p0sCofVtvL_oIeFWNNKGcv9iMdNcwMXXDzGifLIWiQ48hFHkxVInMwZlGnja2s_d_WvL4H0v6n1hcxmdWA3GGn6jMV6d-GX_POXR9hO9uph_XZEpTi7PoWXy1sD6lkIPzr-5dP_L915H9wV0bQQbrS25sQGTV_SiLNRP6rUQrKepRKanOk-bjnvEJU4he9cvr5z5caUHBx0dzFDnJCTVD8sFrYcqLvuy20Uqus58-v-T5mqQfVcEFY9DZFq4rxHOd50h0hvQLM/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit
https://secure-web.cisco.com/1-QRVl4sxcfjWZp6YgOWKAKJzKAlR_7F_l7FBH2DlcrNxj28971TvyG3D9TUY7yjqDSQpFDD1cnUDClMxcS5LTpP2yZTAwaIS0TZaWVPLssYGuKtKb1E0XqENY9Rsfh6_ETm2-nUYG3JD_dMZ2IsaFkhc8gkZ8mttKHmSf7i-6Kp6uRv3mlB43KECYM1LxTVCM82pSlZsp8WEmqWAqKDOL2xJ84gtaQQCIZM7zYrZZN1QEiGHUw5VvY3eT0B7MpjQ_mhtwqJkV4AUGApHdPioxXJ8XxQweNrThd9aGwtrOYaf1lV6zwy9Ub2_nSCbcsN81Tem-OjoMabJVULfpk9qctXstwFam_Z-NakErpuQk7w/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...